Design and fabrication of high-performance diamond triple-gate field-effect transistors
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2016-10-06 |
| Journal | Scientific Reports |
| Authors | Jiangwei Liu, Hirotaka Ohsato, Xi Wang, Meiyong Liao, Yasuo Koide |
| Institutions | National Institute for Materials Science |
| Citations | 52 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Device Innovation: Fabrication of a Hydrogen-terminated diamond (H-diamond) triple-gate MOSFET to overcome the lack of large-area single-crystal diamond wafers and push device downscaling forward.
- Record Output Current: The triple-gate architecture achieves an absolute maximum drain-source current (IDS,max) of 174.2 mA mm-1, approximately 4x higher than the planar-type device (45.2 mA mm-1) fabricated simultaneously on the same substrate.
- Superior Switching Efficiency: Subthreshold swing (SS) is reduced to 110 mV dec-1 (vs. 460 mV dec-1 for planar), attributed to a lower interfacial trap charge density (Dit) of 8.95 × 1011 eV-1 cm-2.
- High On/Off Ratio: Both architectures demonstrate an on/off ratio exceeding 108, confirming viability for practical logic and power applications.
- Reduced On-Resistance: RON drops to 31.9 Ω mm for the triple-gate MOSFET compared to 98.0 Ω mm for the planar counterpart.
- Methodology: Utilizes MPCVD for homoepitaxial H-diamond regrowth on patterned (001) substrates, followed by ICP-RIE fin etching, ALD-deposited Al2O3 gate dielectric, and Pd/Ti/Au ohmic contacts.
- Strategic Value: Establishes diamond as a manufacturable path for high-power, high-frequency, and high-temperature electronics competing with SiC and GaN.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Type | CVD single-crystal diamond (001) | — | Homoepitaxial H-diamond growth |
| Substrate Dimensions | 5.0 × 5.0 × 0.3 | mm | Commercial EDP Corp. wafer |
| Band Gap Energy | 5.47 | eV | Wide-bandgap semiconductor |
| Breakdown Field (theoretical) | 10 | MV cm-1 | High-power capability |
| Thermal Conductivity | 22 | W cm-1 K-1 | Highest among semiconductors |
| Hole Saturation Velocity | 0.85-1.2 × 107 | cm s-1 | High-frequency operation |
| Carrier Mobility (electrons/holes) | 4500 / 3800 | cm2 V-1 s-1 | Theoretical maximum |
| Gate Insulator | Al2O3 | — | ALD-deposited, 27.9 nm thickness |
| Insulator Dielectric Constant | 5.4 | — | Al2O3 permittivity |
| Capacitance (CAl2O3) | 0.171 | µF cm-2 | Calculated from thickness |
| Ohmic Contact | Pd/Ti/Au (10/20/100 nm) | — | E-gun evaporated |
| Gate Leakage (VGS = 30 V) | 1.8 × 10-12 | A | Triple-gate MOSFET |
| Max Drain Current (Triple-gate) | 174.2 | mA mm-1 | IDS,max at optimized VGS |
| Max Drain Current (Planar) | 45.2 | mA mm-1 | Baseline planar MOSFET |
| On-Resistance (Triple-gate) | 31.9 | Ω mm | Linear IDS-VDS extraction |
| On-Resistance (Planar) | 98.0 | Ω mm | Linear IDS-VDS extraction |
| Channel Resistance (RCH) | 23.8 | Ω mm | Fin-patterned channel |
| Source/Drain Resistance (2RSD) | 8.1 | Ω mm | LS/D-G = 500 nm |
| On/Off Ratio | >108 | — | Both architectures |
| Subthreshold Swing (Triple-gate) | 110 | mV dec-1 | At VDS = -10.0 V |
| Subthreshold Swing (Planar) | 460 | mV dec-1 | At VDS = -10.0 V |
| Interfacial Trap Density (Triple-gate) | 8.95 × 1011 | eV-1 cm-2 | From SS equation |
| Interfacial Trap Density (Planar) | 7.14 × 1012 | eV-1 cm-2 | From SS equation |
| Threshold Voltage (Triple-gate) | 10.2 ± 0.1 | V | Depletion-mode operation |
| Threshold Voltage (Planar) | 7.6 ± 0.1 | V | Depletion-mode operation |
| Transconductance (Triple-gate) | 15.3 ± 0.1 | mS mm-1 | Peak extrinsic gm |
| Transconductance (Planar) | 3.8 ± 0.1 | mS mm-1 | Peak extrinsic gm |
| Effective Mobility (Triple-gate) | 6.1 ± 0.5 | cm2 V-1 s-1 | Fin-patterned channel |
| Effective Mobility (Planar) | 38.7 ± 0.5 | cm2 V-1 s-1 | Reference value |
| Cut-off Frequency (Prior Work) | >10 | GHz | Over wide VGS range |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: CVD single-crystal diamond (001) substrate cleaned in H2SO4:HNO3 (1:1) mixed acid at 300 °C for 3 hours.
- W Mask Sputtering: Tungsten layer (200 nm) deposited via automatic sputtering at 300 W in Ar ambient for 30 minutes.
- Photolithography: FEP-171 positive photoresist spin-coated at 5000 rpm for 1 s; baked at 120 °C for 2 min; exposed via EB lithography (ELS-7000); developed in TMAH for 1.5 min.
- W Dry Etching (Bosch Process): ICP-RIE with SF6 (75 sccm, 175 W) and C4F8 (60 sccm, 150 W).
- Diamond Fin Etching: ICP-RIE in O2 ambient (10 sccm, 400 W, 0.5 Pa, 25 min) to form fin-patterned structures.
- Pre-Growth Annealing: Fin-patterned substrate annealed in MPCVD chamber at 1000 °C for 20 min to remove surface contamination.
- H-Diamond Epitaxial Growth (MPCVD):
- System: Seki AX5200S
- Temperature: 900-940 °C
- Chamber Pressure: 80 Torr
- Duration: 20 min
- Gas Flow: H2 at 500 sccm, CH4 at 0.5 sccm
- Mesa Etching: CCP-RIE in O2 (10 Pa, 50 W, 1.5 min) using PMGI-SF6S/FEP-171 bilayer photoresist.
- Ohmic Contact Formation: Pd/Ti/Au (10/20/100 nm) via E-gun evaporation; evaporation rates 0.05/0.05/0.2 nm s-1; chamber pressure 1.0-2.5 × 10-5 Pa.
- Gate Insulator (ALD-Al2O3): Precursors Al(CH3)4 + H2O; pulse/purge 0.1/4.0 s; deposition temperature 120 °C; thickness 27.9 nm.
- Gate Electrode (UHV Sputtering): Al layer at 50 W, 0.3 Pa, Ar 10 sccm, 7 min.
- Al Wet Etching: Mixed acid (H3PO4:HNO3:CH3COOH:H2O = 16:2:2:1) for 1 min.
- Al2O3 Wet Etching: TMAH solution for 10 min.
- Photoresist Stripping: NMP solution at room temperature for 3 hours.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”- Applicable Materials: This research requires Optical Grade Single Crystal Diamond (SCD) substrates in (001) orientation with sub-nanometer surface roughness. 6CCVD supplies high-purity homoepitaxial SCD wafers and H-terminated diamond epitaxial layers grown via MPCVD, directly applicable to replicating or extending this triple-gate MOSFET architecture.
- Custom Substrate Dimensions: The paper utilized 5.0 × 5.0 × 0.3 mm substrates. 6CCVD provides custom SCD plates and wafers up to 125 mm, enabling scaling beyond the constrained small-format substrates that currently limit diamond electronics manufacturing.
- Epitaxial Growth Expertise: 6CCVD’s in-house MPCVD systems deliver precise H-diamond homoepitaxial layers under controlled conditions (H2/CH4 gas ratios, substrate temperatures of 900-940 °C, optimized chamber pressure), replicating the high-quality channel layers essential for low Dit and high hole sheet density.
- Custom Metalization: The Pd/Ti/Au (10/20/100 nm) ohmic stack and Al gate metallization used in this study fall squarely within 6CCVD’s internal metalization capabilities (Au, Pt, Pd, Ti, W, Cu). Custom contact stacks can be deposited via E-gun evaporation or sputtering to match specific work-function and adhesion requirements for source/drain and gate electrodes.
- Surface Engineering: The subthreshold swing of 110 mV dec-1 achieved here hinges on ultra-clean H-diamond surfaces. 6CCVD offers polishing to Ra < 1 nm for SCD and Ra < 5 nm for inch-size PCD, plus acid-cleaning protocols analogous to those described in the methods section.
- Laser Cutting & Patterning: For prototyping fin-array devices, 6CCVD provides laser cutting services to deliver substrates in custom geometries, reducing downstream fabrication complexity for researchers building multi-gate device architectures.
- Engineering Support: 6CCVD’s in-house PhD team can assist with material selection, epitaxial layer thickness optimization, and surface termination strategies (H-, O-, or NO2-treated) for high-power, high-frequency MOSFET and MESFET research. Whether targeting depletion-mode or enhancement-mode operation, 6CCVD provides consultation grounded in semiconductor physics and CVD diamond growth science.
- Call to Action: For custom specifications, H-diamond epitaxial layers, or material consultation on diamond electronic device projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract The lack of large-area single-crystal diamond wafers has led us to downscale diamond electronic devices. Here, we design and fabricate a hydrogenated diamond (H-diamond) triple-gate metal-oxide-semiconductor field-effect transistor (MOSFET) to extend device downscaling and increase device output current. The device’s electrical properties are compared with those of planar-type MOSFETs, which are fabricated simultaneously on the same substrate. The triple-gate MOSFET’s output current (174.2 mA mm −1 ) is much higher than that of the planar-type device (45.2 mA mm −1 ), and the on/off ratio and subthreshold swing are more than 10 8 and as low as 110 mV dec −1 , respectively. The fabrication of these H-diamond triple-gate MOSFETs will drive diamond electronic device development forward towards practical applications.