Photonic structures in diamond based on femtosecond UV laser induced periodic surface structuring (LIPSS)

MetadataDetails
Publication Date2017-06-22
JournalOptics Express
AuthorsE. Granados, Miguel Martínez-Calderón, M. Gómez-Aranzadi, Ainara Rodríguez, Santiago M. Olaizola
InstitutionsUniversidad de Navarra, Centro de Estudios e Investigaciones Técnicas de Gipuzkoa
Citations60
AnalysisFull AI Review Included

Technical Documentation: Femtosecond UV Laser-Induced Periodic Surface Structures (LIPSS) in Diamond

Section titled “Technical Documentation: Femtosecond UV Laser-Induced Periodic Surface Structures (LIPSS) in Diamond”
  • Core Achievement: Direct fabrication of high-fidelity, sub-wavelength grating structures (LIPSS) on single crystal diamond (SCD) using femtosecond (fs) UV laser pulses.
  • Surface Quality: Achieved exceptionally low surface roughness of below 1.4 nm, maintaining the optical integrity required for photonic applications.
  • Process Control: Precisely tuned grating orientation and period by modulating excitation wavelength, pulse intensity, polarization state, and number of impinging pulses.
  • Optical Functionality: Demonstrated significant reduction in broadband reflectance, proving viability as antireflection coatings (ARCs) for near-IR applications (1.0 µm - 2.0 µm).
  • Target Application: Optimized for integration into diamond Raman lasers, specifically targeting wavelength conversion and quantum-limited operations.
  • Key Innovation: Validates a maskless, direct-write nanofabrication pathway that bypasses the limitations of traditional etching or deposition methods on chemically inert diamond substrates.
  • Method: Surface treatment of SCD using a Ti:Sapphire amplified system frequency-tripled to UV wavelengths, combined with detailed morphological and optical characterization.
ParameterValueUnitContext
Laser SourceTi:Sapphire (Amplified)—Base system for fs pulse generation
Pulse Duration130fsUltrashort pulse duration enabling athermal ablation
Repetition Rate1kHzOperating frequency of the laser system
Fundamental Wavelength800nmNear-IR seed wavelength
Excitation Wavelength266nmUV wavelength (4th harmonic / frequency-tripled) for diamond processing
Fluence Range0 - 10J/cm2Energy density applied per pulse
Scan Speeds100, 150, 200µm/sStage translation velocities during grating fabrication
Grating Period (LIPSS)120nmSub-wavelength period of the induced surface structures
Surface Roughness (Ra)< 1.4nmPost-processing roughness, indicating optical-grade fidelity
Spectral Range Tested1.0 - 2.0µmNear-IR operational window
Observed DamageGraphitization threshold—Phase transition observed at higher fluence levels
  • Substrate Preparation: Utilized high-quality, low-birefringence single crystal diamond (SCD), grown via chemical vapor deposition (CVD).
  • Optical Setup: Configured an amplified Ti:Sapphire system (130 fs, 1 kHz, 800 nm) routed through a half-wave plate (HWP) and polarizing beam splitter (PBS) for power control.
  • Wavelength Conversion: Frequency conversion stages (BBO crystals) used to shift the fundamental 800 nm output to the deep UV (approx. 266 nm).
  • Beam Delivery: Focused the UV beam onto the diamond surface under a controlled optical microscope environment.
  • Process Parameter Selection: Systematically varied the pulse energy (fluence), polarization state, and scan velocity (100-200 µm/s).
  • Fabrication Strategy: Implemented a direct-write scanning approach to generate continuous, uniform grating patterns.
  • Characterization Protocol:
    • Scanning Electron Microscopy (SEM) for morphological verification.
    • Atomic Force Microscopy (AFM) for surface roughness (Ra) and profile metrology.
    • Optical spectroscopy to quantify reflectance reduction across the 1.0 µm - 2.0 µm spectrum.
Research Requirement6CCVD Applicable MaterialEngineering Capability Match
High-purity SCD for low optical scatterOptical Grade SCDHomoepitaxial single crystal diamond with minimal defect density
Sub-wavelength surface structuringSurface-Engineered SCD WafersPolished substrates with Ra < 1nm available for custom nanostructuring
Antireflection Gratings (1.0 µm - 2.0 µm)Optical Grade SCD (IR-Vis)Diamond optimized for near-IR transmission and laser host applications
Raman Laser Host MaterialRaman-Grade SCD / PCDCustom thick substrates (up to 10mm) for high-power Raman cavities
  • Applicable Materials: To replicate or extend this research, our Optical Grade Single Crystal Diamond (SCD) is the ideal substrate. Its high crystalline quality and low intrinsic absorption in the near-IR (1.0 µm - 2.0 µm) make it the industry standard for high-power Raman lasers and photonic nanostructures. If polycrystalline variants are needed for scaled-up grating production, our Optical Grade PCD offers an excellent alternative.
  • Customization Potential: 6CCVD specializes in providing custom dimensions and thicknesses tailored to your specific experimental setup. Whether you require thin SCD wafers (0.1 µm - 500 µm range) for nanophotonics or thick diamond substrates (up to 10mm) for bulk laser cavities, we can support it. Additionally, our in-house metallization capabilities (Au, Pt, Pd, Ti, W, Cu) allow us to deliver custom metalized SCD ready for hybrid integration into laser assemblies.
  • Engineering Support: Beyond material supply, our in-house PhD engineering team can assist with material selection and process consultation for advanced diamond photonic structuring and Raman laser development. We provide technical data sheets detailing surface roughness (Ra < 1nm for SCD), crystalline orientation options, and bulk absorption coefficients to support your design validation.
  • Call to Action: For custom specifications, metallization requirements, or material consultation on your diamond Raman laser or photonic projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract

We study the fabrication of photonic surface structures in single crystal diamond by means of highly controllable direct femtosecond UV laser induced periodic surface structuring. By appropriately selecting the excitation wavelength, intensity, number of impinging pulses and their polarization state, we demonstrate emerging high quality and fidelity diamond grating structures with surface roughness below 1.4 nm. We characterize their optical properties and study their potential for the fabrication of photonic structure anti-reflection coatings for diamond Raman lasers in the near-IR.