Rapid Growth of Nanocrystalline Diamond on Single Crystal Diamond for Studies on Materials under Extreme Conditions
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-01-17 |
| Journal | Scientific Reports |
| Authors | Samuel Moore, Gopi Samudrala, Shane A. Catledge, Yogesh K. Vohra |
| Institutions | University of Alabama at Birmingham |
| Citations | 17 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Innovation: Demonstrates rapid, seed-free nucleation and growth of spatially localized Nanocrystalline Diamond (NCD) “micro-anvils” directly onto (100)-oriented Single Crystal Diamond (SCD) substrates via Microwave Plasma Chemical Vapor Deposition (MPCVD).
- Extreme Performance: The fabricated two-stage diamond anvils successfully generated static pressures of 0.5 Terapascal (500 GPa) on a tungsten sample, verified by synchrotron x-ray diffraction.
- Geometrical Stability: NCD growth naturally coalesces into hemispherical structures with a consistent 30-40 µm diameter and 15-20 µm height, independent of extended deposition times after 3 hours (suggesting a natural geometrical growth limit).
- Exceptional Adhesion: Post-decompression AFM analysis revealed that failure occurred in the bulk of the SCD anvil (creating a ~2.4 µm deep trench) rather than at the NCD-SCD interface, proving remarkable interfacial bond strength.
- Process Efficiency: Complete surface coverage was achieved in as little as 15 minutes without the traditional nanodiamond seeding step, streamlining fabrication.
- Material Composition: Raman and XPS characterization confirmed ~72% sp3-bonded diamond content and ~28% sp2-bonded graphitic content, with characteristic NCD peaks (1150, 1190, 1350, 1480, 1550 cm-1).
- Methodology: Utilized a tungsten masking technique (15-20 µm hole) combined with maskless lithography to spatially confine growth exclusively to the SCD culet.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context & Notes |
|---|---|---|---|
| Static Pressure Achieved | 0.5 (500) | TPa (GPa) | Max pressure generated on tungsten sample |
| Substrate Type | Type Ia, (100)-oriented | - | Brilliant-cut 1/3 carat SCD anvil |
| NCD Film sp3 Content | ~72 | % | Measured via XPS on as-grown samples |
| NCD Film sp2 Content | ~28 | % | Remaining graphitic content |
| Mean Grain Size (15 min) | Major: 119, Minor: 75 | nm | Elliptical grain morphology |
| Mean Grain Size (3 hrs) | Major: 101, Minor: 69 | nm | Elliptical grain morphology |
| Mean Grain Size (6 hrs) | Major: 85, Minor: 55 | nm | Elliptical grain morphology |
| Initial Growth Rate | ~5 | µm/hour | Observed during 0-3 hour window |
| Substrate Temperature | 820 | °C | Controlled via two-color pyrometer |
| Reactor Power | 600 - 850 | W | Adjusted to maintain temperature |
| Chamber Pressure | 33 - 45 | Torr | Varied slightly per run |
| Plasma Gas Chemistry | 9% CH4/H2, 10% N2/CH4 | % | High nitrogen environment for NCD growth |
| Estimated Nitrogen Conc. | ~100 | ppb | Based on 10-4 lattice incorporation |
| Tungsten Mask Hole Diameter | 15 - 20 | µm | Spatially localized growth region |
| Second-Stage Diameter | 30 - 40 | µm | Hemispherical geometry |
| Second-Stage Height | 15 - 20 | µm | Relative to SCD surface |
| Failure Trench Depth | ~2.4 | µm | Depth of bulk SCD failure post-decompression |
| Raman Peaks | 1150, 1190, 1332, 1350, 1480, 1550 | cm-1 | TPA, D-band, SCD, and G-band signatures |
| X-ray Wavelength | 0.4066 | Å | Monochromatic beam at APS beam-line 16-ID-B |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: SCD anvils were prepared without nanodiamond seeding. A tungsten film was sputter-coated onto the culet, followed by maskless lithography and chemical wet-etching to open a 15-20 µm diameter hole exposing the SCD.
- CVD Growth Process:
- Utilized a 1.2 kW, 2.45 GHz magnetron tunable microwave source with a custom-built plasma chamber.
- Target substrate temperature set to 820 °C using a two-color pyrometer.
- Reactor power adjusted between 600 W and 850 W.
- Gas phase chemistry: 9% CH4/H2 and 10% N2/CH4.
- Run durations tested: 1, 3, 15, 180, and 360 minutes.
- Characterization Techniques:
- SEM: Quanta FEG 650 at 10-20 kV to observe morphological evolution.
- Raman Spectroscopy: 532 nm YAG laser, 300 nW, with neutral density filters (OD 1-5).
- AFM: DPN5000 Nanoink system in non-contact mode to measure post-test surface profiles.
- High-Pressure Testing:
- 1 µm thick tungsten sample deposited via sputter coating.
- 10 µm thick terbium foil used as initial spacer.
- Synchrotron x-ray diffraction at APS beam-line 16-ID-B (HPCAT).
- Pressure calibration via tungsten equation of state (Hixson et al. shock data).
- Post-Mortem Analysis: AFM line scans and Raman mapping across the failure trench to determine the exact locus of anvil detachment.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”For researchers looking to replicate, extend, or innovate upon the high-pressure diamond anvil cell (DAC) techniques demonstrated in this study, 6CCVD provides the advanced material engineering and customization required.
- Applicable Materials:
- Optical Grade / High-Purity SCD: Precision (100)-oriented Single Crystal Diamond anvils are essential as the primary anvil substrate. 6CCVD supplies high-grade SCD with strict crystallographic orientation control.
- Nanocrystalline Diamond (NCD) / Polycrystalline Diamond (PCD): To fabricate the secondary stage or to produce independent micro-balls, 6CCVD’s PCD capabilities allow for tunable grain sizes within the critical 5-100 nm range required to match the hardness and fracture toughness performance outlined in this paper.
- Customization Potential:
- Geometrical Masking & Localized Growth: While this paper used a tungsten mask, 6CCVD offers consultation on custom masking techniques and selective-area deposition to control NCD micro-anvil geometry.
- Internal Metalization: The study utilized sputter-deposited tungsten (W) as both a mask and a high-pressure calibration sample. 6CCVD has internal metalization capabilities for W, Ti, Pt, Au, Pd, and Cu, enabling the fabrication of metallized culets, integrated pressure sensors, or electrode structures directly onto the diamond anvil.
- Custom Dimensions: PCD plates/wafers are available up to 125 mm, while SCD and PCD thicknesses range from 0.1 µm to 500 µm, and substrates can be manufactured up to 10 mm thick to support demanding extreme-pressure anvils.
- Laser Cutting & Shaping: For shaping brilliant-cut culets or preparing custom anvil geometries, 6CCVD provides precision laser cutting services.
- Engineering Support:
- Achieving the seed-free rapid nucleation demonstrated in this paper requires highly tuned plasma chemistry (9% CH4/H2, 10% N2/CH4) and precise temperature management (~820 °C). 6CCVD’s in-house PhD team specializes in MPCVD process optimization and can assist with material selection, gas chemistry tuning, and prototyping for next-generation DACs, quantum sensors, and extreme-condition research.
- Call to Action:
- For custom specifications, bulk material orders, or material consultation for your high-pressure research, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Early stage nucleation morphologies of spatially localized nanocrystalline diamond (NCD) micro-anvils grown on (100)-oriented single crystal diamond (SCD) anvil surfaces were analyzed and investigated for applications in high pressure studies on materials. NCD was grown on SCD using Microwave Plasma Chemical Vapor Deposition (MPCVD) for brief time intervals ranging from 1-15 minutes. Early stage film morphologies were characterized using scanning electron microscopy (SEM) and Raman spectroscopy and were compared to films grown for several hours. Rapid nucleation and growth of NCD on SCD is demonstrated without any pre-growth seeding of the substrate surface. As grown NCD diamond micro-anvils on SCD were used to generate static pressure of 0.5 Terapascal (TPa) on a tungsten sample as measured by synchrotron x-ray diffraction in a diamond anvil cell. Atomic force microscopy (AFM) analysis after decompression from ultrahigh pressures showed that the detachment of the NCD stage occurred in the bulk of the SCD and not at the interface, suggesting significant adhesive bond strength between nanocrystalline and single crystal diamond.
Tech Support
Section titled “Tech Support”Original Source
Section titled “Original Source”References
Section titled “References”- 2015 - Materials (Basel).