Minority carrier lifetime in ultrananocrystalline diamond/hydrogenated amorphous carbon composite films
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-11-30 |
| Journal | Transactions of the Materials Research Society of Japan |
| Authors | Naofumi Nishikawa, Satoshi Takeichi, Takanori Hanada, Shuya Tategami, Atsuhiko Fukuyama |
| Institutions | University of Miyazaki, Kyushu University |
| Citations | 3 |
| Analysis | Full AI Review Included |
Technical Documentation: Minority Carrier Lifetime in UNCD/a-C:H Composite Films
Section titled “Technical Documentation: Minority Carrier Lifetime in UNCD/a-C:H Composite Films”Executive Summary
Section titled “Executive Summary”- Material Innovation: The study investigates ultrananocrystalline diamond (UNCD)/hydrogenated amorphous carbon (a-C:H) composite films, characterized by diamond crystallites <10 nm embedded in an a-C:H matrix with extensive grain boundaries (GBs).
- Hydrogenation Impact: Hydrogen termination of dangling bonds at GBs effectively passivates carrier trap centers, increasing minority carrier lifetime (τSRH) from 0.21 µs (UNCD/a-C) to 0.43 µs (UNCD/a-C:H) — a >2× enhancement.
- Photovoltaic Validation: pn heterojunction diodes (p-type UNCD/a-C:H / n-type Si) exhibit enhanced photocurrent with increased hydrogen content, validating τ measurements as a predictor of UV photodetector performance.
- Deposition Method: Films were synthesized via Coaxial Arc Plasma Deposition (CAPD) at 550°C under 53.3 Pa hydrogen pressure, with arc discharge voltage tuning (70-115 V) to control hydrogen incorporation.
- Carrier Transport: Ideality factors of 2-3 indicate tunneling-assisted generation-recombination (G-R) mechanisms, consistent with variable-range hopping (VRH) transport in highly disordered GB networks.
- Application Potential: Large absorption coefficients across 3-6 eV photon range position these films as candidates for deep-UV photovoltaic sensors and harsh-environment photodetectors.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Temperature | 550 | °C | CAPD deposition for UNCD/a-C:H |
| Hydrogen Pressure (H2) | 53.3 | Pa | Process atmosphere |
| Base Pressure (UNCD/a-C) | < 10-4 | Pa | Non-hydrogenated reference |
| Arc Discharge Capacitance | 720 | µF | Coaxial arc plasma gun |
| Arc Discharge Voltage Range | 70-115 | V | Tuning parameter for H content |
| Pulse Repetition Rate | 5 | Hz | Arc discharge frequency |
| Target-to-Substrate Distance | 15 | mm | Geometric configuration |
| UNCD Grain Diameter | < 10 | nm | Crystallite size |
| Boron Doping (p-type film) | 0.5 | at.% | Heterojunction diode |
| Si Substrate Resistivity | 1-5 | Ω·cm | n-type (100) Si |
| Si Substrate Thickness | 260 | µm | Heterojunction substrate |
| τSRH (UNCD/a-C:H) | 0.43 | µs | Hydrogenated composite |
| τSRH (UNCD/a-C) | 0.21 | µs | Non-hydrogenated composite |
| τAuger (UNCD/a-C:H) | 0.07 | µs | Fast decay component |
| τAuger (UNCD/a-C) | 0.02 | µs | Fast decay component |
| τSRH-trapping (UNCD/a-C:H) | 5.16 | µs | Slow decay component |
| τSRH-trapping (UNCD/a-C) | 1.58 | µs | Slow decay component |
| Laser Wavelength (µ-PCD) | 349 | nm | Excess carrier generation |
| Laser Pulse Duration | 5 | ns | Excitation source |
| Microwave Frequency | 26 | GHz | Reflectivity probe |
| Ideality Factor | 2-3 | — | Diode forward current |
| UV Irradiation Wavelength | 254 | nm | Photocurrent measurement |
Key Methodologies
Section titled “Key Methodologies”- Film Synthesis (CAPD)
- Graphite target sputtered via coaxial arc plasma gun (Ulvac ARL-300).
- Substrate: insulating single-crystalline Si (>10 kΩ·cm resistivity).
- Hydrogen content controlled by varying arc discharge voltage (70, 85, 100, 115 V) under fixed 53.3 Pa H2.
- Boron Doping for pn Junction
- 0.5 at.% boron introduced into UNCD/a-C:H films during CAPD to achieve p-type conduction.
- Heterojunction formed on n-type Si (1-5 Ω·cm, 260 µm).
- Electrode Fabrication
- Palladium (Pd) top contact via RF magnetron sputtering.
- Aluminum (Al) back contact via RF magnetron sputtering.
- Minority Carrier Lifetime Measurement (µ-PCD)
- Microwave-reflected photoconductivity decay (KOBELCO LTA-1512EP).
- 349 nm laser pulse (5 ns) generates excess carriers.
- Differential microwave reflectivity (26 GHz) tracks decay kinetics.
- Three-component fitting: Auger, SRH, and SRH-with-trapping.
- Device Characterization
- I-V measurements in dark and under 254 nm UV irradiation.
- Ideality factor extraction from forward-bias current.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”The UNCD/a-C:H composite system requires a specialized polycrystalline diamond with controlled sp2/sp3 content and grain boundary engineering. For research groups seeking to replicate or extend this work on UNCD-based UV photodetectors, the following 6CCVD materials are directly applicable:
- Optical Grade PCD — Fine-grained polycrystalline diamond suitable for UV photodetector substrates, offering tunable grain boundary densities and proven optical absorption characteristics across the visible-to-UV spectrum.
- Heavy Boron-Doped PCD (BDD) — Matches the 0.5 at.% boron doping level reported in this paper for p-type conduction; available with custom resistivity profiles.
- Nanocrystalline Diamond Films — 6CCVD’s MPCVD platform can deposit nanocrystalline and ultrananocrystalline diamond (UNCD) with grain sizes <10 nm, directly analogous to the UNCD phase in this composite system.
Customization Potential
Section titled “Customization Potential”This research employs a Pd/Al metallization stack on 260 µm Si substrates. 6CCVD’s in-house capabilities align precisely:
| Research Requirement | 6CCVD Capability |
|---|---|
| Pd top electrode | Palladium (Pd) metallization — RF magnetron sputtering available |
| Al back contact | Aluminum, Ti, Au, Pt, W, Cu — full metallization portfolio |
| UNCD/a-C:H composite deposition | Custom MPCVD recipes — tunable CH4/H2/Ar plasma chemistry for nanocrystalline grain control |
| Substrate flexibility | Wafers up to 125 mm (PCD); custom substrates available |
| Film thickness control | 0.1-500 µm (SCD/PCD) and up to 10 mm substrates |
Laser cutting and dicing services are available for device fabrication and chip singulation, supporting pn heterojunction diode prototyping.
Engineering Support
Section titled “Engineering Support”For teams developing UNCD-based UV photovoltaic sensors, deep-UV photodetectors, or pn heterojunction devices, the following support pathway is available:
- In-house PhD engineering team with expertise in MPCVD process optimization, grain boundary engineering, and boron-doping calibration.
- Material consultation for selecting optimal grain size, sp2 content, and hydrogen incorporation strategies to maximize minority carrier lifetime.
- Custom deposition parameter development — including substrate temperature (up to 950°C), plasma power tuning, and gas chemistry optimization for UNCD/a-C:H composite film synthesis.
- Characterization support guidance — advice on µ-PCD measurements, I-V characterization, and ideality factor analysis for novel diamond heterostructures.
Call to Action
Section titled “Call to Action”For custom specifications, metallization stack design, or material consultation on UNCD/a-C:H composite films and diamond-based UV photovoltaic devices, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Ultrananocrystalline diamond (UNCD)/hydrogenated amorphous carbon (a-C:H) composite (UNCD/a-C:H) films possess the following specific characteristics: (a) the appearance of additional energy levels in diamond bandgap and (b) large absorption coefficients ranging from visible to ultraviolet, both of which might be due to large number of grain boundaries between UNCD grains and those between UNCD grains and a-C:H. Owing to them, UNCD/a-C:H films are expected to be applied to photovoltaics such as UV sensors. Actually thus far, we have fabricated pn heterojunction diodes comprising p-type UNCD/a-C:H films and n-type Si substrates, and confirmed their photovoltaic action. In this study, the minority carrier lifetime, which is an important factor for photovoltaics, was experimentally measured by microwave reflected photoconductivity decay, and it was estimated to be 0.21 and 0.43 μs for UNCD/a-C and UNCD/a-C:H, respectively. In addition, on the basis of the previous work on the heterojunctions, the effects of hydrogenation on the photovoltaic action of the heterojunctions were studied. The photocurrent apparently increases with an enhancement in the hydrogenation of UNCD/a-C:H films, which might be because dangling bonds in the UNCD/a-C:H films, which act as photogenerated-carrier trap centers, are terminated by hydrogen atoms.