Observation of a superconducting glass state in granular superconducting diamond
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2019-03-14 |
| Journal | Scientific Reports |
| Authors | Georgina M. Klemencic, J. M. Fellows, Jessica M. Werrell, Soumen Mandal, S. R. Giblin |
| Institutions | University of Bristol, University of Birmingham |
| Citations | 3 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Material System: Nanocrystalline boron-doped diamond (BNCD) thin films grown by MPCVD on 500 nm SiO2/Si substrates.
- Superconducting Behavior: Reports the first clear evidence of a “superconducting glass state” in granular superconducting diamond, characterized by a quasi de Almeida-Thouless (AT) irreversibility line and logarithmic magnetic relaxation.
- Phase Boundary Mapping: Uses quasi-zero-dimensional fluctuation conductivity theory to define the H-T phase boundary with higher precision than standard onset/midpoint/offset criteria.
- Critical Parameters: Tc > 4 K; carrier concentration between 1 × 1021 cm-3 and 2.3 × 1021 cm-3; film thickness 564 nm; mean grain diameter 102 ± 24 nm.
- Granularity Control: Film morphology (grain size, granularity) is identified as the primary driver of glassy vortex dynamics, with thickness acting as a tunable structural lever.
- Measurement Stack: Four-wire Van der Pauw transport + vibrating sample magnetometry in a Quantum Design PPMS, with field perpendicular to the film plane.
- Significance: Provides a new framework for interpreting disorder-driven superconductivity in doped diamond and similar granular low-Tc systems.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate | 500 nm SiO2-buffered (100) Si | — | 2″ diameter wafer |
| Film thickness | 564 | nm | BNCD superconducting film |
| Mean grain diameter | 102 ± 24 | nm | Determined by SEM |
| Surface roughness (RMS) | ~45 | nm | Pre-polishing |
| Growth temperature | ~720 | °C | Substrate temperature during MPCVD |
| Methane concentration | 3 | % | In H2 carrier gas |
| Boron source | Trimethylboron (TMB) | — | B/C ratio 12,800 ppm |
| Chamber pressure | 40 | Torr | MPCVD process |
| Microwave power | 3.5 | kW | Plasma generation |
| Carrier concentration | >1 × 1021 (up to 2.3 × 1021) | cm-3 | Estimated from gas-phase B/C ratio |
| Superconducting Tc (onset) | ~4 | K | Zero-resistance state reached ~2 K |
| Measurement temperature range | 1.4 - 4.5 | K | PPMS cryostat |
| Magnetic relaxation regime | 2.2 | K | Logarithmic decay observed |
| Irreversibility line fit | Hirr ∝ (1 − T/Tc)3/2 | — | Quasi de Almeida-Thouless behavior |
| Transport geometry | 4-wire Van der Pauw | — | Silver paste contacts |
| Magnetometry | VSM, field ⊥ plane | — | Quantum Design PPMS |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation
- Use of a (100) silicon wafer with a 500 nm thermal SiO2 buffer layer.
- Ultrasonic seeding in a monodisperse aqueous colloid of 5 nm nanodiamond particles to generate a high-density nucleation layer, ensuring uniform, fully coalesced nanocrystalline film growth.
- MPCVD Film Growth
- Substrate temperature stabilized at ~720 °C.
- Process gas: 3% CH4 in H2 with TMB as boron precursor.
- B/C gas-phase ratio: 12,800 ppm.
- Chamber pressure: 40 Torr; microwave power: 3.5 kW.
- Film Characterization
- Thickness: 564 nm (cross-sectional SEM).
- Grain size: 102 ± 24 nm (plan-view SEM).
- RMS roughness: ~45 nm; prior work shows polishing does not alter superconducting transition.
- Electrical Transport
- Four-wire Van der Pauw configuration using silver paste contacts.
- Resistance vs. temperature recorded across 1.4-4.5 K under perpendicular magnetic fields.
- Magnetic Measurements
- Vibrating sample magnetometry (VSM) on a Quantum Design PPMS.
- DC magnetization recorded as a function of field and temperature to map irreversibility.
- Time-dependent relaxation measurements performed at 2.2 K to confirm logarithmic magnetic decay.
- Phase Boundary Analysis
- Application of quasi-zero-dimensional fluctuation conductivity theory to fit resistive transitions.
- Extraction of Hirr(T) and comparison against the AT line Hirr ∝ (1 − T/Tc)3/2.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
- The study requires a Heavy Boron-Doped Polycrystalline Diamond (BDD) in the metallic regime of the metal-insulator transition (carrier density >1021 cm-3).
- 6CCVD’s high-pressure MPCVD reactors deliver Polycrystalline Diamond (PCD) with controlled grain size and boron incorporation suitable for reproducing this granular superconductor platform.
- Nanocrystalline-grade PCD (sub-100 nm grain morphology) can be specified to match the 102 ± 24 nm grain diameter reported, preserving the weakly coupled cluster network essential to glassy vortex dynamics.
Customization Potential
- The authors used a 564 nm film on a 2″ SiO2/Si wafer. 6CCVD routinely delivers custom thicknesses from 0.1 µm to 500 µm for both SCD and PCD, enabling systematic thickness-dependent studies of granularity-driven superconductivity.
- Wafer-scale plates up to 125 mm (PCD) and custom die dimensions are available, ideal for Van der Pauw or Hall-bar device patterning.
- For four-wire contact preparation, 6CCVD provides in-house metalization with Ti, Pt, Au, Pd, W, or Cu (e.g., Ti/Pt/Au stacks) and laser-cutting/structuring services to deliver ready-to-measure chips.
- For studies where surface morphology must be controlled independently of superconductivity, 6CCVD’s PCD polishing down to Ra < 5 nm (inch-size) can be applied without degrading the doped layer.
Engineering Support
- 6CCVD’s in-house PhD engineering team can assist with selecting the optimal boron concentration, grain morphology, and thickness to target a specific Tc or carrier density window for quantum transport, NEMS, or vortex-matter research.
- We provide consultation on CVD recipe tuning (CH4/H2 ratios, TMB flow, pressure, microwave power) to dial in the precise metallic-regime doping required for granular superconductivity experiments.
- For multi-parameter studies—such as thickness-dependent irreversibility line mapping—6CCVD can supply matched sample sets with consistent boron incorporation but varying grain size or thickness.
Call to Action
For custom specifications, matched sample sets, or material consultation on boron-doped diamond for superconductivity and quantum device research, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
The magnetic field dependence of the superconductivity in nanocrystalline boron doped diamond thin films is reported. Evidence of a superconducting glass state is presented, as demonstrated by the observation of a quasi de Almeida-Thouless line in the phase diagram and a logarithmic time dependence of the magnetism. The position of the phase boundary in the H-T plane is determined from electrical transport data by detailed fitting to quasi-zero-dimensional fluctuation conductivity theory. This allows determination of the boundary between resistive and non-resistive behaviour to be made with greater precision than the standard ad hoc onset/midpoint/offset criterion. We attribute the glassy superconductivity to the morphological granularity of the diamond films.