Fabrication of Capacitive Pressure Sensor Using Single Crystal Diamond Cantilever Beam: Technical Documentation

Section titled “Fabrication of Capacitive Pressure Sensor Using Single Crystal Diamond Cantilever Beam: Technical Documentation”
  • Core Innovation: Successful fabrication of a micro-electromechanical (MEMS) capacitive pressure sensor utilizing a freestanding single crystal diamond (SCD) cantilever beam on an HPHT diamond substrate.
  • Substrate & Epitaxy: Fabrication began with an HPHT Ib (001) SCD substrate, modified using 3 MeV selective carbon ion implantation, followed by homoepitaxial layer growth via Microwave Plasma Chemical Vapor Deposition (MPCVD) at 1175 °C.
  • Microfabrication Process: The beam structures were defined using photolithography and a 1 µm aluminum hard mask, followed by Inductively Coupled Plasma (ICP) etching and non-contact electrochemical etching to release the sacrificial graphite layer.
  • Electrode Patterning: Tungsten (W) metal was deposited via evaporation to form the capacitive electrodes, specifically tailored to two test geometries (65 µm and 95 µm long cantilevers with 2.5 µm thicknesses).
  • Mechanical & Electrical Performance: Atomic Force Microscopy (AFM) force-displacement (F-w) measurements validated mechanical integrity without fracture. Capacitance-voltage (C-V) characterization was executed using an Agilent B1505A parameter analyzer across 50 kHz to 1 MHz.
  • Performance Metrics: Sensitivity increases with larger electrode surface area and decreases with higher measurement frequency (50 kHz to 1 MHz).
  • Application Horizon: Demonstrates the viability of SCD for high-sensitivity, stable pressure monitoring in extreme environments (high temperature, high radiation, strong corrosion) where standard silicon sensors fail.
ParameterValueUnitContext
Substrate TypeHPHT Ib (001)—Base material for ion implantation
Ion Implantation Energy3MeVCarbon ions for sacrificial layer creation
MPCVD Growth Temperature1175°CHomoepitaxial layer deposition
Aluminum Mask Thickness1µmHard mask for ICP etching
Cantilever Thickness2.5µmStructural depth of the MEMS device
Cantilever Width30µmUniform across all test structures
Cantilever Length (Array)65, 95, 125, 155µmTest bed variations
Electrode Area A35 × 30µm²Capacitive electrode on shorter cantilever
Electrode Area B50 × 30µm²Capacitive electrode on longer cantilever
Electrode MaterialTungsten (W)—Deposited via thermal evaporation
Capacitive Air Gap~40nmMeasured vertical displacement range
Measurement Frequencies50, 100, 1000 (1M)kHzC-V curve characterization range
Force Loading Range0 to ~4µNApplied via AFM tip
Applied Voltage Sweep-4 to +4VCapacitance-voltage measurement window
  • Substrate Preparation: Utilized HPHT Ib (001) single crystal diamond substrate as the foundation.
  • Sacrificial Layer Generation: Performed selective high-energy ion implantation with carbon ions at 3 MeV to create a damaged subsurface layer.
  • Epitaxial Growth: Conducted homoepitaxial diamond growth using a Microwave Plasma Chemical Vapor Deposition (MPCVD) system at 1175 °C, which converts the damaged layer into a graphite sacrificial layer.
  • Masking: Deposited a 1 µm thick aluminum film via magnetron sputtering, then patterned it using conventional photolithography to define the beam geometries.
  • Bulk Micromachining: Executed Inductively Coupled Plasma (ICP) etching through the aluminum mask to reach the sacrificial layer.
  • Release Process: Applied a non-contact electrochemical etching system to selectively remove the buried graphite layer, releasing the freestanding SCD cantilever beam.
  • Electrode Fabrication: Utilized photolithography and metal evaporation to deposit tungsten (W) electrode patterns on the cantilever and substrate surfaces.
  • Characterization:
    • Measured mechanical displacement vs. force loading using Atomic Force Microscopy (AFM).
    • Measured capacitance-voltage (C-V) characteristics using an Agilent B1505A parameter analyzer.
  • Applicable Materials:
    • To replicate the substrate foundation, Optical Grade Single Crystal Diamond (SCD) wafers are required. 6CCVD can supply HPHT Ib (001) substrates and high-purity homoepitaxial SCD layers grown via MPCVD, free of grain boundaries to ensure the mechanical integrity and superior electronic properties demonstrated in the paper.
    • For applications demanding larger device footprints (beyond standard 3x3mm or 5x5mm research pieces), 6CCVD offers custom SCD plates and substrates up to 125mm diameter for scaling sensor arrays.
  • Customization Potential:
    • The paper utilizes Tungsten (W) for the electrode metallization. 6CCVD features in-house metallization capabilities (including Ti, W, Pt, Au, Pd, and Cu) and can provide custom lift-off or patterned evaporation services to match specific MEMS design requirements.
    • Custom thicknesses are available. To achieve the 2.5 µm beam thickness noted in the study, 6CCCD provides precision lapping and polishing of SCD down to sub-micron tolerances (Ra < 1nm surface roughness).
  • Engineering Support:
    • Transitioning SCD-based pressure sensors from laboratory scale to commercial production requires precision material integration. 6CCVD’s in-house PhD engineering team can assist with material selection, defect analysis, and metallization stack design for next-generation MEMS devices intended for harsh environment sensing (aerospace, nuclear, and combustion chambers).
  • Call to Action:
    • For custom specifications, metallization consultation, or to request a quote on SCD substrates tailored for MEMS fabrication, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract

Fabrication of single crystal diamond capacitive pressure sensor is presented. Firstly, the single crystal diamond cantilever beam was formed on HPHT diamond substrate by using selective high-energy ion implantation, metal patterning, ICP etching and electrochemical etching techniques. Secondly, on this diamond cantilever beam, the desired electrode patterns were processed with photolithography and metal evaporation methods. Furthermore, the displacements of cantilever beam under different pressure conditions were investigated by atomic force microscopy. The capacitance-voltage curves of single crystal diamond cantilever beam and substrate under different force loading conditions were measured by using Agilent B1505A parameter analyzer. The results show that sensitivity increases with the enlargement of electrode area of cantilever beam, and decreases with the rise of measurement frequency.