High-Q Diamond Microresonators in the Long-Wave Infrared: Technical Documentation
Section titled “High-Q Diamond Microresonators in the Long-Wave Infrared: Technical Documentation”Executive Summary
Section titled “Executive Summary”- Breakthrough Demonstration: First reported whispering-gallery mode (WGM) single-crystal diamond (SCD) microdisk resonators operating in the deeper long-wave infrared (LWIR), specifically across the 9-9.7 µm spectral range.
- Record Quality Factors: Achieved Q factors exceeding 3000 (measured values of 3648 at 9.601 µm and 3130 at 9.541 µm), surpassing the prior state-of-the-art in this wavelength range by more than an order of magnitude.
- Fabrication Innovation: Utilized oxygen-based inductively coupled plasma reactive ion etching (ICP RIE) at angled profiles to create protruding ring waveguides on millimeter-scale SCD substrates.
- Spectral Validation: Fourier analysis confirmed free spectral ranges (FSR) slightly greater than 40 GHz, matching theoretical expectations for the microresonator geometry and diamond’s refractive index.
- Material Selection Rationale: Diamond selected over germanium, zinc selenide, and potassium bromide due to superior transparency and lower absorption losses beyond 9 µm.
- Optical Characterization Setup: Tested at room temperature using a tunable quantum cascade laser (QCL) coupled via free space, with light extracted through an As2Se3 chalcogenide fiber to a cryogenically cooled HgCdTe detector.
- Application Impact: Establishes a pathway for high-Q photonic devices in the 8-14 µm thermal infrared region, critical for sensing, thermal imaging, and spectroscopy applications.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Operating Wavelength Range | 9.0 - 9.7 | µm | Deeper LWIR spectral region |
| Peak Resonance Wavelength (Disk 1) | 9.601 | µm | High-Q resonance demonstration |
| Peak Resonance Wavelength (Disk 2) | 9.541 | µm | Second device confirmation |
| Quality Factor (Q) - Device 1 | 3648 | - | Measured at 9.601 µm |
| Quality Factor (Q) - Device 2 | 3130 | - | Measured at 9.541 µm |
| Free Spectral Range (Theoretical) | ~40 | GHz | Calculated for n ≈ 2.4 |
| Free Spectral Range (Measured) | slightly >40 | GHz | Confirmed via Fourier analysis |
| FSR (Wavenumber) | ~1.33 | cm−1 | Theoretical value at 9.5 µm |
| Refractive Index (Diamond) | 2.4 | - | At ~9.5 µm wavelength |
| QCL Scan Rate | 0.1 | cm−1/s | Spectral measurement parameter |
| Disk Diameter | Millimeter-scale | mm | Fabrication target size |
| Minimum Q Improvement vs. Prior Art | >10× | - | Compared to existing LWIR cavities |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Single-crystal diamond (SCD) substrates selected for low absorption in the 8-12 µm thermal infrared window.
- Mask Patterning: Photolithography performed to define microdisk resonator geometry on the diamond surface.
- Hard Mask Deposition: SiNx layer deposited via HDPCVD (high-density plasma chemical vapor deposition) to serve as etch mask.
- ICP RIE SiNx: Initial patterning of the hard mask using inductively coupled plasma reactive ion etching.
- Angled ICP RIE on SCD: Oxygen-based plasma chemistry employed at high incident angles to create slanted sidewall profiles and protruding ring waveguide structures.
- Mask Removal: SiNx hard mask stripped using buffered oxide etch (BOE).
- Optical Characterization: Tunable quantum cascade laser (QCL) scanned across 9-9.7 µm range with free-space coupling into resonators.
- Signal Extraction: As2Se3 chalcogenide infrared fiber directed transmitted light to a cryogenically cooled HgCdTe detector.
- Data Processing: Lock-in amplifier detection with Fourier transform analysis to verify FSR consistency with theoretical predictions.
- Quality Factor Extraction: Lorentzian curve fitting of resonance lineshapes to determine Q values.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”| Research Requirement | Recommended 6CCVD Product |
|---|---|
| Low-loss single-crystal diamond for LWIR photonics | Optical Grade SCD (Single Crystal Diamond) - High-purity substrates with minimal nitrogen content |
| Millimeter-scale resonator fabrication | SCD Plates/Wafers up to 125mm - Custom dimensions available |
| Ultra-smooth surface for low scattering losses | SCD with Ra < 1nm polishing - Sub-nanometer surface finish achievable |
| Thin-film flexibility for various geometries | SCD thickness range 0.1µm - 500µm - Supports diverse device architectures |
Customization Potential
Section titled “Customization Potential”- Precision Laser Cutting: 6CCVD offers laser cutting services to produce custom microdisk diameters and geometries matching the millimeter-scale resonator specifications used in this study.
- Advanced Polishing: For extending this research toward even higher Q factors, our sub-nanometer Ra polishing capability (Ra < 1nm for SCD) minimizes sidewall roughness scattering—the primary loss mechanism in WGM resonators.
- Thickness Optimization: Custom SCD thicknesses from 0.1µm to 500µm enable optimization of evanescent field overlap and mode confinement for specific LWIR wavelengths.
- Material Purity Control: Tailored nitrogen concentration (< 5 ppb available) for minimizing absorption losses in the 9-12 µm window.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD engineering team specializes in diamond material selection for advanced photonics applications including:
- Whispering-gallery mode (WGM) resonators
- Long-wave infrared (LWIR) optical devices
- Quantum cascade laser (QCL) integration platforms
- Thermal infrared sensing and spectroscopy systems
- MEMS and microfabricated diamond structures
Our team can provide guidance on optimal substrate orientation (e.g., (100) vs. (111)), crystal quality grades, and surface preparation protocols to replicate or extend the high-Q performance demonstrated in this work.
Call to Action
Section titled “Call to Action”For custom specifications, material consultation, or technical collaboration on long-wave infrared diamond photonic devices, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
High quality factor (Q) photonic devices in the room temperature thermal infrared region, corresponding to deeper long-wave infrared with wavelengths beyond 9 microns, have been demonstrated for the first time. Whispering gallery mode diamond microresonators were fabricated using single crystal diamond substrates and oxygen-based inductively coupled plasma (ICP) reactive ion etching (RIE) at high angles. The spectral characteristics of the devices were probed at room temperature using a tunable quantum cascade laser that was free space-coupled into the resonators. Light was extracted via an arsenic selenide (As 2 Se 3 ) chalcogenide infrared fiber and directed to a cryogenically cooled mercury cadmium telluride (HgCdTe) detector. The quality factors were tested in multiple microresonators across a wide spectral range from 9 to 9.7 microns with similar performance. One example resonance (of many comparables) was found to reach 3648 at 9.601 µm. Fourier analysis of the many resonances of each device showed free spectral ranges slightly greater than 40 GHz, matching theoretical expectations for the microresonator diameter and the overlap of the whispering gallery mode with the diamond.