Fabrication of electrolyte-gate nanocrystalline diamond- based field effect transistor (NCD-EGFET) for HIV-1 Tat protein detection
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2020-02-01 |
| Journal | IOP Conference Series Materials Science and Engineering |
| Authors | Nurul Atiqah Ahmad, A. Rahim Ruslinda, Nur Syakimah Ismail, Bohuslav Rezek |
| Institutions | Czech Academy of Sciences, Institute of Physics, Universiti Malaysia Perlis |
| Citations | 1 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Device Fabricated: Electrolyte-Gate Field Effect Transistor (EGFET) utilizing nanocrystalline diamond (NCD) as the transducing material on a silicon substrate for biosensing applications.
- Target Application: Label-free detection of HIV-1 Tat protein via RNA aptamer functionalization.
- Transducer Material Advantage: NCD offers biocompatibility, surface wettability, high stability, and surface conductivity post-hydrogenation.
- Detection Performance: Demonstrated a highly reproducible gate potential shift of ~174 mV upon binding of 100 pM HIV-1 Tat protein.
- Fabrication Method: Microwave ellipsoidal cavity CVD reactor followed by standard photolithographic patterning (mark, channel, contact, and cover alignment).
- Channel Geometry: Active gate channels defined with 60 µm length and 20 µm width, terminated with hydrogen bonding for surface conductivity.
- Significance: Validates NCD as a robust, biocompatible semiconductor platform for next-generation electrochemical biosensors operating in wet/physiological conditions.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Material | Silicon (Si/SiO2) | — | 10 mm × 10 mm × 1 mm oxidized wafer |
| Active Transducer | Nanocrystalline Diamond (NCD) | — | Grown via MPCVD |
| Diamond Film Thickness | ~450 | nm | Deposition duration 4.5 h |
| Diamond Grain Size | ~250 | nm | Determined via SEM analysis |
| Nucleation Particle Size | 4.8 ± 0.6 | nm | Buckydiamond in NanoAmando solution |
| Nucleation Layer Thickness | 5-25 | nm | Ultrasonic seeding layer |
| CH4 Concentration in H2 | 1 | % | Gas mixture ratio |
| Deposition Pressure | 30 | mbar | Process chamber vacuum |
| Microwave Power | 1000 | W | Ellipsoidal cavity reactor |
| Deposition Temperature | 550-600 | °C | Substrate temperature |
| Hydrogenation Temperature | 600 | °C | Surface conductivity activation |
| Hydrogenation Duration | 10 | min | H2 plasma treatment |
| Gate Channel Length | 60 | µm | Photolithographic patterning |
| Gate Channel Width | 20 | µm | Photolithographic patterning |
| Contact Adhesion Layer | Titanium (Ti) | 10 nm | E-beam/sputter deposition |
| Contact Conductive Layer | Gold (Au) | 50 nm | Biocompatible electrode |
| Reference Electrode | Ag/AgCl | — | Gate terminal in electrolyte |
| Electrolyte | 1 mM PBS | pH 7.4 | Physiological measurement buffer |
| Target Analyte | HIV-1 Tat Protein | 100 pM | Specific binding partner |
| Recognition Probe | RNA Aptamer | — | Functionalized on gate surface |
| Detection Signal (ΔVg) | ~174 | mV | Negative shift upon binding |
| Isoelectric Point (Tat) | 9.88 | pI | Confirms positive charge at pH 7.4 |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Oxidize 10 mm × 10 mm × 1 mm silicon substrates in an oxidation furnace to form a SiO2 barrier layer.
- Substrate Cleaning: Ultrasonicate in isopropyl alcohol (10 min), rinse with DI water.
- Nanopowder Nucleation: Ultrasonic bath for 30-40 min in a colloidal suspension (200 mL DIW + 5 mL NanoAmando 5.0 w/v% diamond nanopowder) to seed the growth surface.
- MPCVD Diamond Deposition: Grow NCD thin film in a microwave ellipsoidal cavity reactor for 4.5 hours.
- Pressure: 30 mbar
- Gas Mixture: 1% CH4 in H2
- Microwave Power: 1000 W
- Substrate Temperature: 550-600 °C
- Surface Conductivity Activation: Hydrogenate NCD film in H2 plasma at 600 °C for 10 min within the same MPCVD reactor.
- Photolithographic Mark Alignment: Spin-coat HDMS (1:4) at 3000 rpm for 10 sec; spin-coat positive photoresist (MA 15) at 3000 rpm for 30 sec; soft-bake at 100 °C for 2 min.
- UV Exposure & Development: Align under mask aligner, expose to UV for 6 sec, develop for 45 sec, and oxygen plasma clean for 1 min.
- Metal Contact Deposition: Deposit 10 nm Ti adhesion layer followed by 50 nm Au via physical vapor deposition.
- Lift-Off: Remove excess metal in acetone to define alignment marks.
- Channel & Contact Patterning: Repeat photolithography process to define the 60 µm × 20 µm active gate channel and source/drain contact pads.
- Final Passivation/Cover: Pattern a dielectric cover layer (e.g., SU-8 or polyimide) to isolate contact pads and expose only the active gate area to the electrolyte.
- Biofunctionalization: Immobilize RNA aptamer specific to HIV-1 Tat onto the hydrogen-terminated NCD active gate channel.
- Electrical Measurement: Measure Ids-Vgs transfer characteristics using a Keithley 2400 Source Meter and 6487 Picoammeter with an Ag/AgCl reference gate electrode.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”The fabrication of high-sensitivity EGFET biosensors requires extremely uniform diamond films with precise control over surface termination, doping, and grain boundary morphology. Below is how 6CCVD’s capabilities align with the requirements of this research.
Applicable Materials
Section titled “Applicable Materials”- Nanocrystalline Diamond (NCD) Films: The paper utilized NCD grown via MPCVD with a 1% CH4/H2 recipe at 30 mbar and 1000 W. 6CCVD routinely manufactures custom NCD and Polycrystalline Diamond (PCD) wafers up to 125 mm diameter, capable of replicating and scaling this exact nanocrystalline morphology.
- Surface-Terminated Diamond: The hydrogen-terminated surface (H-diamond) is critical for inducing p-type surface conductivity via electrolyte gating. 6CCVD provides hydrogenated diamond wafers with ultra-low surface roughness (Ra < 5 nm for inch-size PCD), ensuring uniform electrostatic potential across the 60 µm × 20 µm channel architecture.
- Ultra-Thin Film Capability: The paper utilized a ~450 nm thick film. 6CCVD offers diamond thickness ranges from 0.1 µm to 500 µm, enabling researchers to optimize transducer capacitance and minimize charge screening effects for future device iterations.
Customization Potential
Section titled “Customization Potential”- Custom Metalization: The paper relies on a 10 nm Ti / 50 nm Au contact stack. 6CCVD offers in-house custom metalization using Au, Pt, Pd, Ti, W, and Cu. We can provide patterned metal contacts directly on your diamond substrates, eliminating the need for in-house lithography and PVD systems.
- Laser Cutting & Dicing: While the paper used 10 mm × 10 mm Si chips, 6CCVD provides laser-cut custom geometries down to specific micron-level channels, enabling rapid prototyping of novel FET architectures.
- Wafer-Scale Production: Scaling up from single 10 mm chips to full 100 mm or 125 mm wafers introduces challenges with film uniformity and defect density. 6CCVD’s MPCVD reactors are optimized for high-uniformity, wafer-scale diamond deposition required for multiplexed biosensor arrays.
Engineering Support
Section titled “Engineering Support”Navigating the transition from a single-device laboratory demonstration (a single 174 mV response to HIV-1 Tat) to a clinically viable diagnostic requires deep materials expertise. 6CCVD’s in-house PhD engineering team specializes in MPCVD process optimization, surface chemistry, and carrier transport in diamond. We assist clients in selecting the optimal diamond grade—whether it be Optical Grade SCD for fundamental studies or specialized PCD for scalable electrochemical arrays—for projects spanning biosensing, quantum sensing, and power electronics. Our team can help you engineer the grain boundary density, sp2/sp3 ratio, and surface termination energy to maximize your device’s sensitivity and limit of detection.
For custom specifications, wafer-scale material consultation, or to request a quote on patterned diamond wafers, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract In this paper, we reported on the fabrication process of electrolyte-gate field effect transistor using nanocrystalline diamond as a sensing transducer. The fabrication procedure was begin with the growth of nanocrystalline diamond thin film on silicon/silicon dioxide (Si/SiO 2 ) substrate using microwave plasma-enhanced chemical vapour deposition (CVD). Then the photolithography process was performed in order to design and pattern the field effect transistor device with the active gate channel of 60 µm length and 20 µm width. Each device consists of three active gate channel which connecting to three different pairs of source and drain contact. The surface morphology of fabricated NCD-EGFET was characterized using Scanning Electron Microscope to clarify the active gate channel of the device and the grain size of nanocrystaline diamond. The current-voltage ( I-V ) measurement of the device were carried out to study the electrical behaviour for HIV-1 Tat protein detection via RNA aptamer as sensing probe.