Specific surface defects arising from diamond CVD-synthesis from methane-hydrogen plasma
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2020-09-01 |
| Journal | IOP Conference Series Materials Science and Engineering |
| Authors | T. V. Martynova, N. I. Polushin, А. I. Laptev, Е. С. Захарова, A L Maslov |
| Institutions | National University of Science and Technology |
| Citations | 1 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Objective: Systematic identification and characterization of surface defects on Single Crystal Diamond (SCD) films grown via Microwave Plasma Chemical Vapor Deposition (MPCVD) for photonics and microelectronics applications.
- Material System: SCD CVD-films, 300-500 µm thick, homoepitaxially grown on [100]-oriented substrates.
- Key Process Parameters: 3% CH4/H2 plasma; substrate temperature 1100 °C; microwave power 3800 W; chamber pressure 33.3 kPa; demonstrated growth rate up to 28 µm/h.
- Substrate Quality: Misorientation angle ≤ 1.5°; nitrogen impurity ≤ 5 ppm (FTIR verified).
- Three Primary Defect Classes Identified:
- Etch pits — localized crystallographic voids in the growth zone.
- “Straying” diamonds — isolated polycrystalline particles nucleating on the growth surface.
- Peripheral coarse-grained diamond — polycrystalline overgrowth along substrate edges.
- Root Cause Analysis: Defect density correlates strongly with high growth rate, elevated CH4 concentration, and substrate imperfections (misorientation, surface roughness, contamination).
- Proposed Mitigation: Substrate preparation (precision polishing, O2/H2 plasma etching), process parameter optimization, and periodic defect removal (mechanical, chemical, or laser-based).
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context / Notes |
|---|---|---|---|
| Film Type | Single Crystal Diamond (SCD) | — | Homoepitaxial CVD film |
| Film Thickness | 300 - 500 | µm | Final processed thickness |
| Maximum Growth Rate | 28 | µm/h | Demonstrated under cited conditions |
| Methane Concentration (CH4) | 3 | % | In H2 carrier gas |
| Hydrogen Purity | 99.999 (% / 5.5) | — | Carrier gas grade |
| Methane Purity | 99.995 (% / 4.5) | — | Source gas grade |
| Substrate Temperature | 1100 | °C | During deposition |
| Microwave Power | 3800 | W | Plasma excitation |
| Chamber Pressure | 33.3 | kPa | Total system pressure |
| Substrate Orientation | [100] | — | Crystallographic direction |
| Substrate Misorientation | ≤ 1.5 | ° | Off-axis angle |
| Substrate N Content | ≤ 5 | ppm | Measured via FTIR |
| Defect Type 1 | Etch pits | — | Surface voids |
| Defect Type 2 | ”Straying” diamonds | — | Isolated polycrystalline particles |
| Defect Type 3 | Peripheral polycrystalline rim | — | Coarse-grained edge overgrowth |
| Surface Characterization | SEM | — | Morphological analysis |
Key Methodologies
Section titled “Key Methodologies”-
Substrate Preparation
- Single crystal diamond substrates, [100] orientation.
- Misorientation angle controlled to ≤ 1.5°.
- Substrates verified for low nitrogen content (≤ 5 ppm) via Fourier-Transform Infrared Spectroscopy (FTIR).
-
MPCVD Growth Process
- Gas mixture: 3% CH4 in H2 (purity grades 4.5 and 5.5 respectively).
- Substrate temperature maintained at 1100 °C.
- Microwave radiation power: 3800 W.
- Total chamber pressure: 33.3 kPa.
- Deposition duration tuned to yield 300-500 µm thick films.
-
Surface Defect Characterization
- Scanning Electron Microscopy (SEM) used to image and classify surface morphology.
- Three defect categories catalogued: etch pits, stray diamond particles, peripheral polycrystalline overgrowth.
-
Defect Mitigation Strategy (Proposed)
- Pre-growth substrate polishing to defined misorientation angles.
- Oxygen-hydrogen plasma etching of substrates prior to deposition.
- Optimization of gas phase composition, temperature, pressure, and gas flow rate.
- Sectoral growth control to suppress polycrystalline nucleation.
- Periodic mechanical, chemical, or laser-based removal of emerging defects, followed by chemo-thermal etching and regrowth.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials:
- Optical/Electronic Grade SCD: For researchers replicating this work, 6CCVD provides high-purity Single Crystal Diamond (SCD) plates and wafers with controlled nitrogen content (sub-ppm to low-ppm range), grown via MPCVD on [100]-oriented substrates with tight misorientation control.
- Substrates for Homoepitaxy: Low-nitrogen, precision-polished SCD substrates (misorientation ≤ 1.5°) suitable for homoepitaxial CVD regrowth cycles.
- Ultra-Thick SCD Films: Stock thicknesses from 0.1 µm to 500 µm available; custom CVD overgrowth services for films exceeding 500 µm to support thick-window and high-energy physics applications.
Customization Potential:
- The paper highlights that defect formation is strongly tied to substrate edge effects and peripheral polycrystalline overgrowth. 6CCVD offers laser cutting and custom shaping to deliver edge-finished, near-net-shape diamond plates, minimizing edge-nucleation sites before re-entry into the CVD chamber.
- For experiments requiring patterned or metallized growth surfaces, 6CCVD’s in-house metalization capabilities (Ti, Pt, Au, Pd, W, Cu) enable pre-structured substrates for selective area growth or in-situ device integration.
- Custom wafer dimensions up to 125 mm (PCD) and tailored SCD geometries are available to support scaled reactor campaigns.
Engineering Support:
- 6CCVD’s in-house PhD engineering team can assist with material selection, substrate specification, and process parameter mapping for homoepitaxial SCD overgrowth, photonics, and microelectronics projects targeting ultra-low defect density.
- Consultation available on trade-offs between growth rate (e.g., 28 µm/h regime vs. slower high-quality regimes), methane fraction, and resulting defect populations, as well as chemo-thermal polishing and surface preparation protocols to extend or replicate this research.
Call to Action: For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract Diamond is unique material that have long been known to humanity. It has extra high hardness, thermal conductivity, as well as unique electrophysical characteristics that can be managed by changing its impurity composition. Therefore, this material has gained the potential of widespread use in engineering, which is currently complicated by the high cost of diamonds, difficulties of its synthesis, mechanical and physical processing. A promising direction for obtaining high-quality poly- and single crystals and, accordingly, expanding the areas of diamond use is the method of its deposition from the gas phase (CVD). The main problem that researchers face during deposition the diamond is the formation of surface defects in the growth zone. In this work, we discuss defects observed on single-crystal diamond CVD-films of 300-500 μm thick obtained from methane-hydrogen plasma with 3% methane. The surface was studied by scanning electron microscopy. As a result of the work, we revealed that during the diamond films CVD-growth mainly three types of defects are formed: etch pits, isolated diamond particles (“straying” diamonds) and coarse-grained diamond formed along the diamond plates periphery. Methods for eliminating these defects are proposed.