Preparation and characterization of AFM tips with nitrogen-vacancy and nitrogen-vacancy-nitrogen color centers
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2021-06-30 |
| Journal | Photonics Letters of Poland |
| Authors | Zuzanna Orzechowska, Mariusz Mrózek, Wojciech Gawlik, Adam M. Wojciechowski |
| Institutions | Laboratoire d’Informatique de Paris-Nord, Photonics (United States) |
| Citations | 1 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Objective: Develop a simple, cost-effective dip-coating method to functionalize standard silicon AFM probes with fluorescent nanodiamonds (NDs) for combined AFM/fluorescence imaging and spatially resolved magnetometry.
- Material Used: Commercial nanodiamond powder (Adamas Nanotechnologies MDNVN1µm) with a mean particle size of ~750 nm, containing ~2 ppm NVN (H3) centers and ~0.1 ppm NV centers.
- Coating Process: Dip-coating of PPP-CONTR silicon AFM cantilevers (tip height 10-15 µm) into an isopropyl alcohol ND suspension, with two repetitions typically required to ensure sufficient NV-rich crystal attachment.
- Key Innovation: Enables optical visualization of AFM tips above transparent samples and converts standard probes into scanning magnetometers without requiring custom diamond tip fabrication.
- Detection Scheme: Wide-field fluorescence microscopy using 532 nm green laser excitation, with NV/NVN emissions filtered using a 600 nm long-pass filter and imaged on a CMOS camera.
- ODMR Demonstration: Microwave-driven spin resonance of NV centers measured around 2.87 GHz, with Zeeman shifts observed under external magnetic fields from 0 to 1.0 mT, confirming magnetic field sensing capability.
- Advantage: Bridges standard silicon AFM technology with quantum sensing by leveraging ensemble NV/NVN color centers in nanodiamonds rather than requiring single-defect diamond scanning probes.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| AFM probe type | PPP-CONTR (Nanosensors) | — | Standard silicon probe used as substrate |
| Chip dimensions | 3.4 × 1.4 × 0.3 | mm | Overall probe chip size |
| Cantilever thickness | 2.0 ± 0.1 | µm | Silicon cantilever thickness |
| Cantilever length | 450 ± 10 | µm | Standard PPP-CONTR geometry |
| Cantilever width | 50 ± 7.5 | µm | Standard PPP-CONTR geometry |
| Tip height | 10-15 | µm | Distance from chip base to apex |
| Nanodiamond type | MDNVN1µm (Adamas Nanotechnologies) | — | Fluorescent ND powder |
| ND mean particle size | ~750 | nm | Average crystal dimension |
| NV center concentration | ~0.1 | ppm | Concentration in ND powder |
| NVN (H3) center concentration | ~2 | ppm | Concentration in ND powder |
| Suspension medium | Isopropyl alcohol | — | Solvent for dip-coating |
| Dip-coating repetitions | 2 (typical) | cycles | Required for sufficient NV-rich crystal density |
| Excitation wavelength (NV) | 532 | nm | Green laser source |
| Excitation wavelength (NVN) | Blue light | nm | Blue excitation for NVN centers |
| Laser output power | 60 | mW | Max power at fiber output (532-L-OE-115-1W) |
| Beam diameter (expanded) | ~9 | mm | Collimated beam diameter |
| Objective magnification / NA | 40× / 0.6 | — | Olympus LUCPLFLN |
| Fluorescence filter | 600 nm long-pass | nm | FEL0600 (Thorlabs) |
| Detector | CMOS camera | — | Wide-field fluorescence imaging |
| ODMR MW frequency | ~2.87 | GHz | NV ground-state spin resonance |
| Fluorescence contrast (ODMR dip) | ~1-10 | % | Typical dip depth on resonance |
| Magnetic field test range | 0-1.0 | mT | Applied field steps (0, 0.3, 0.5, 0.7, 1.0 mT) |
| MW frequency sweep range | 2820-2920 | MHz | ODMR spectrum window |
Key Methodologies
Section titled “Key Methodologies”- Probe Selection: Use commercial PPP-CONTR silicon AFM probes with well-characterized geometry (450 µm cantilever length, 10-15 µm tip height).
- Nanodiamond Suspension: Prepare ND suspension using MDNVN1µm powder (~750 nm crystals) dispersed in isopropyl alcohol at room temperature.
- Dip-Coating Procedure: Carefully immerse the AFM tip into the ND/IPA suspension for a few seconds; withdraw and allow to dry in air; repeat the dip cycle twice for adequate NV-density coverage.
- Fluorescence Imaging Setup: Assemble a wide-field microscope with a 532 nm green laser (60 mW), 40× NA 0.6 objective, dichroic mirror (DMLP567), and 600 nm long-pass emission filter; image onto a CMOS camera.
- ODMR Configuration: Apply microwave field near 2.87 GHz via an MW antenna near the cantilever while monitoring fluorescence; sweep MW frequency from 2820-2920 MHz.
- Magnetic Field Calibration: Record ODMR spectra at discrete applied magnetic fields (0, 0.3, 0.5, 0.7, 1.0 mT) to confirm Zeeman shifts and validate magnetometry capability.
- Verification: Visually confirm under the microscope that fluorescence from individual ND crystals is dominated by either NV (red) or NVN (green) emission, ensuring that dip cycles yield sufficient fluorescent particles near the tip apex for high spatial resolution.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”| Paper Requirement | Recommended 6CCVD Solution |
|---|---|
| ~750 nm fluorescent nanodiamonds with NV/NVN centers | Sub-micron to micron-sized Single Crystal Diamond (SCD) particles or engineered nanodiamond powders with controlled NV/NVN density |
| Substrate-independent ND attachment on sharp probes | Custom MPCVD-grown SCD tips mounted on cantilevers, eliminating dip-coating variability entirely |
| High-resolution magnetometry with small crystal-to-source distance | Optical Grade SCD or Boron-Doped Diamond (BDD) crystals with engineered NV ensemble layers grown directly via MPCVD |
| Defined crystal geometry for controlled tip-sample separation | Custom SCD/PCD plates up to 125 mm (PCD) and 500 µm thick (SCD/PCD), diced via laser cutting to specified dimensions |
| Smooth, well-defined emitter surfaces | SCD with Ra < 1 nm polish for high photon extraction efficiency and reproducible ODMR contrast |
| Integrated metallization for MW antennas or electrodes | In-house Ti / Pt / Au / W / Cu metallization on diamond substrates for spin-manipulation electrodes |
Applicable Materials:
For replicating or extending this NV/NVN magnetometry-on-AFM work, the following 6CCVD offerings are directly applicable:
- Optical Grade Single Crystal Diamond (SCD): Provides ultra-low defect background with controlled NV/NVN implantation density, ideal as the active sensing crystal.
- Heavy Boron-Doped Polycrystalline Diamond (BDD): Useful where conductive diamond electrodes are needed for integrated MW delivery or electrostatic control.
- Engineered SCD/PCD Plates (0.1 µm - 500 µm thickness): Thin crystals suitable for bonding onto AFM cantilevers as direct diamond scanning probes, replacing dip-coating with deterministic placement.
Customization Potential:
The dip-coating approach in this paper introduces randomness in crystal placement and orientation. 6CCVD addresses this limitation by offering laser-cutting and dicing services to produce nanodiamond or SCD blocks at precise dimensions, plus custom metallization (Ti/Pt/Au, W, Cu) for monolithic integration of MW antennas directly onto the diamond sensing element — eliminating the need for an external antenna loop.
Engineering Support:
6CCVD’s in-house PhD team can assist with material selection — including NV/NVN density optimization, crystal geometry for tip-apex integration, and metallization stack design — for quantum-sensing AFM, scanning magnetometry, and related quantum metrology projects.
Call to Action:
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We demonstrate a simple dip-coating method of covering standard AFM tips with nanodiamonds containing color centers. Such coating enables convenient visualization of AFM tips above transparent samples as well as using the tip for performing spatially resolved magnetometry. Full Text: PDF ReferencesG. Binnig, C. F. Quate, C. Gerber, “Atomic Force Microscope”, Phys. Rev. Lett. 56, 930 (1986). CrossRef F .J. Giessibl, “Advances in atomic force microscopy”, Rev. Mod. Phys. 75, 949 (2003). CrossRef S. Kasas, G. Dietler, “Probing nanomechanical properties from biomolecules to living cells”, Eur. J. Appl. Physiol. 456, 13 (2008). CrossRef C. Roduit et al., “Stiffness Tomography by Atomic Force Microscopy”, Biophys. J. 97, 674 (2009). CrossRef L. A. Kolodny et al., “Spatially Correlated Fluorescence/AFM of Individual Nanosized Particles and Biomolecules”, Anal. Chem. 73, 1959 (2001). CrossRef L. Rondin et al., “Magnetometry with nitrogen-vacancy defects in diamond”, Rep. Prog. Phys. 77, 056503 (2014). CrossRef C. L. Degen, “Scanning magnetic field microscope with a diamond single-spin sensor”, Appl. Phys. Lett. 92, 243111 (2008). CrossRef J. M. Taylor et al., “High-sensitivity diamond magnetometer with nanoscale resolution”, Nat. Phys. 4, 810 (2008). CrossRef J. R. Maze et al., “Nanoscale magnetic sensing with an individual electronic spin in diamond”, Nature 455, 644 (2008). CrossRef L. Rondin et al., “Nanoscale magnetic field mapping with a single spin scanning probe magnetometer”, Appl. Phys. Lett. 100, 153118 (2012). CrossRef J. P. Tetienne et al., “Nanoscale imaging and control of domain-wall hopping with a nitrogen-vacancy center microscope”, Science 344, 1366 (2014). CrossRef R. Nelz et al., “Color center fluorescence and spin manipulation in single crystal, pyramidal diamond tips”, Appl. Phys. Lett. 109, 193105 (2016). CrossRef G. Balasubramanian et al., “Nanoscale imaging magnetometry with diamond spins under ambient conditions”, Nature 455, 648 (2008). CrossRef P. Maletinsky et al., “A robust scanning diamond sensor for nanoscale imaging with single nitrogen-vacancy centres”, Nat. nanotechnol. 7, 320 (2012). CrossRef L. Thiel et al., “Quantitative nanoscale vortex imaging using a cryogenic quantum magnetometer”, Nat. nanotechnol. 11, 677 (2016). CrossRef F. Jelezko et al., “Single spin states in a defect center resolved by optical spectroscopy”, Appl. Phys. Lett. 81, 2160 (2002). CrossRef M. W. Doherty et al., “The nitrogen-vacancy colour centre in diamond”, Phys. Rep. 528, 1 (2013). CrossRef C. Kurtsiefer, S. Mayer, P. Zarda, H. Weinfurter, “Stable Solid-State Source of Single Photons”, Phys. Rev. Lett. 85, 290 (2000). CrossRef A. Gruber, A. Dräbenstedt, C. Tietz, L. Fleury, J. Wrachtrup, C. Von Borczyskowski, “Scanning Confocal Optical Microscopy and Magnetic Resonance on Single Defect Centers”, Science 276, 2012 (1997). CrossRef F. Dolde et al., “Electric-field sensing using single diamond spins”, Nat. Phys. 7, 459 (2011). CrossRef K. Sasaki et al., “Broadband, large-area microwave antenna for optically detected magnetic resonance of nitrogen-vacancy centers in diamond”, Rev. Sci. Instrum. 87, 053904 (2016). CrossRef A. M. Wojciechowski et al., “Optical Magnetometry Based on Nanodiamonds with Nitrogen-Vacancy Color Centers”, Materials 12, 2951 (2019). CrossRef I. V. Fedotov et al., “Fiber-optic magnetometry with randomly oriented spins”, Opt. Lett. 39, 6755 (2014). CrossRef