Study on the Fabrication and Characteristics of H-Terminated Diamond Bidirectional Switch Devices
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2026-01-01 |
| Journal | Acta Physica Sinica |
| Authors | Yuanchen Ma, Xinyu Yue, Zeyang Ren, Qihui Xu, Jinfeng Zhang |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- First-of-its-kind device: A depletion-mode, common-drain, anti-series monolithically integrated bidirectional switch MOSFET was fabricated on hydrogen-terminated (100) single-crystal diamond (SCD).
- Record electrical performance: Achieved an on/off ratio of 109 and a threshold voltage of 52.8 V, demonstrating excellent gate control and ultra-low gate leakage on a diamond platform.
- Low on-resistance bidirectional conduction: Maximum output currents of 180.52 mA/mm and 170.90 mA/mm with corresponding on-resistances of 0.20 kΩ·mm and 0.23 kΩ·mm in the first and third quadrants.
- High breakdown voltage: Gate-drain breakdown voltages of -358 V and 366 V at a 16 µm gate-drain spacing, yielding a breakdown field of approximately 0.22 MV/cm.
- Key fabrication innovation: A 100 nm Al2O3 layer deposited by ALD at 300 °C serves simultaneously as gate dielectric and surface passivation layer, stabilizing the hydrogen-terminated 2D hole gas (2DHG).
- Surface conductivity activation: Hydrogen plasma treatment in an MPCVD reactor (600 sccm H2, 40 mbar, 1 kW, 650 °C, 30 min) creates the conductive surface channel that outperforms conventional boron-doped channels in on-resistance.
- Application scope: Validates diamond as a viable platform for AC/DC power switching, photovoltaic inverters, EV motor drives, and bidirectional solid-state breakers.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Crystal orientation | (100) | — | Substrate orientation |
| Substrate dimensions | 7 × 7 | mm | CVD-grown SCD substrate |
| Substrate thickness | 0.5 | mm | Bulk diamond thickness |
| Surface termination | H-terminated | — | 2DHG activation |
| Ohmic contact metal | Au (100 nm) | nm | E-beam evaporated |
| Gate dielectric | Al2O3 | — | ALD-grown at 300 °C |
| Dielectric thickness | 100 | nm | Gate + passivation layer |
| Gate metal | Al | — | Lift-off patterned |
| Gate length LG1 | 1.842 | µm | Photolithography-defined |
| Gate length LG2 | 1.733 | µm | Photolithography-defined |
| Gate-source LG1S1 | 4.98 | µm | Device geometry |
| Gate-source LG2S2 | 3.25 | µm | Device geometry |
| Inter-gate LG1G2 | 4.99 | µm | Anti-series spacing |
| Source-source LS1S2 | 16.79 | µm | Channel length |
| Gate width WG1 = WG2 | 100 | µm | Gate finger width |
| On/off ratio (Ion/Ioff) | 109 | — | Transfer curve @ VDS = -20 V |
| Threshold voltage (Vth) | 52.8 | V | Depletion-mode device |
| Max output current (Q1) | 180.52 | mA/mm | Bidirectional conduction |
| Max output current (Q3) | 170.90 | mA/mm | Bidirectional conduction |
| On-resistance (Q1) | 0.20 | kΩ·mm | Bidirectional conduction |
| On-resistance (Q3) | 0.23 | kΩ·mm | Bidirectional conduction |
| Max current (unidirectional) | 175.64 / -205.04 | mA/mm | Single-gate mode |
| On-resistance (unidirectional) | 0.28 / 0.27 | kΩ·mm | Single-gate mode |
| Breakdown voltage VBR (G1) | -358 | V | Gate-drain, G1 shorted to S |
| Breakdown voltage VBR (G2) | 366 | V | Gate-drain, G2 shorted to S |
| Breakdown field | ~0.22 | MV/cm | At 16 µm spacing |
| Measurement instrument | Keysight B1500A | — | Semiconductor parameter analyzer |
| Test temperature | Room temperature | °C | All electrical characterization |
Key Methodologies
Section titled “Key Methodologies”- Substrate preparation: Use CVD-grown (100) single-crystal diamond (7 mm × 7 mm × 0.5 mm) supplied by Shanghai Zhengshi Technology.
- Hydrogen plasma treatment: Expose the cleaned diamond to H2 plasma in an MPCVD chamber to form the hydrogen-terminated conductive surface.
- MPCVD process recipe: H2 flow 600 sccm, chamber pressure 40 mbar, microwave power 1 kW, substrate temperature 650 °C, duration 30 min.
- Ohmic contact deposition: Electron-beam evaporation of 100 nm Au layer as both ohmic electrode and H-surface protective cap.
- Active area definition: Photolithography followed by wet etching in KI/I2 solution to pattern source/drain regions.
- Gate dielectric deposition: Atomic layer deposition (ALD) of 100 nm Al2O3 at 300 °C, functioning simultaneously as gate insulator and surface passivation.
- Gate electrode formation: Al evaporation combined with photolithography and lift-off to define dual gate fingers.
- Electrical characterization: Transfer curves (VGS sweep), output curves (VDS ±40 V, VGS step 10 V), and breakdown measurements on Keysight B1500A at room temperature.
- Operating mode verification: Test three configurations — dual-gate shorted (bidirectional), single-gate shorted to source (unidirectional forward), and reverse unidirectional.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”| Paper Requirement | 6CCVD Offering | Fit for Your Project |
|---|---|---|
| (100) SCD substrate, 7 × 7 mm | Custom SCD up to 125 mm equivalent PCD; SCD plates in optical-grade surface quality | Scalable to research and pilot-line wafer sizes |
| Au ohmic contact, 100 nm | In-house Au, Pt, Pd, Ti, W, Cu metallization | Replace Au-only stack with Ti/Au or Ti/Pt/Au to eliminate metal lift-off at high VDS |
| H-termination for 2DHG | MPCVD H2 plasma activation service | Reproduce 650 °C / 40 mbar / 600 sccm recipe or optimize for your geometry |
| 100 nm Al2O3 by ALD | Polished SCD surfaces Ra < 1 nm ready for downstream dielectric deposition | Atomically smooth interface = lower gate leakage and higher Vth stability |
| Sub-micron photolithography alignment | Laser-cutting and custom patterning services | Minimize LG1/LG2 mismatch that caused Q1/Q3 asymmetry in the paper |
| Au adhesion failure at breakdown | Ti/Au or Ti/Pt/Au metallization stack | Directly addresses the metal “blow-off” failure mechanism reported in the paper |
| > 10 mm substrate for larger area devices | SCD/PCD substrates up to 10 mm thickness | Support future high-voltage designs targeting > 3 MV/cm fields |
Applicable Materials
Section titled “Applicable Materials”For replicating or extending this research, 6CCVD recommends:
- Optical Grade SCD (single-crystal diamond), (100) orientation — matches the substrate used by the authors and is the foundation of the H-terminated 2DHG. Available with Ra < 1 nm surface finish to ensure high-quality Al2O3 interfaces and reproducible threshold voltages.
- Polycrystalline diamond (PCD) alternative — for cost-driven scaling or larger-area demonstrators, where the H-termination route can be transferred to high-grade PCD films grown on 6CCVD substrates up to 125 mm.
Customization Potential
Section titled “Customization Potential”The paper itself flags Ti/Au metallization as the next-step improvement to replace pure Au and eliminate the electrode blow-off observed during breakdown testing. 6CCVD delivers exactly this:
- Custom multilayer metallization: Ti / Au, Ti / Pt / Au, or any stack from the supported metal set (Au, Pt, Pd, Ti, W, Cu), deposited in-house with thickness control from a few nm to several hundred nm.
- Laser cutting and dicing: Tight dimensional control to bring the LG1/LG2 asymmetry (which produced the 180 vs 171 mA/mm current mismatch) to negligible levels.
- Custom thickness: SCD thickness from 0.1 µm to 500 µm, or up to 10 mm substrates for high-voltage stand-off designs targeting the > 3 MV/cm regime the authors outline as future work.
- Wafer-scale H-termination: Process development support for large-area surface conductivity activation.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD engineering team routinely supports customers building diamond power MOSFETs, bidirectional switches, and H-terminated 2DHG devices for EV inverters, photovoltaic converters, and solid-state breakers. We can assist with:
- Material selection between optical-grade SCD and high-quality PCD for your specific voltage/current targets.
- Surface preparation protocol transfer to ensure reproducible 2DHG sheet resistance.
- Metallization stack design (Ti/Au vs Ti/Pt/Au vs W-based) optimized for adhesion and high-field reliability.
- Roadmap planning from laboratory 7 × 7 mm demonstrators to pilot-scale larger-area devices.
Call to Action: For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
双向开关器件在光伏、能源、电动汽车等领域应用广泛,金刚石优异的物理特性有望满足开关器件对低导通电阻和高击穿电压的应用需求。本研究率先采用(100)晶面的氢终端金刚石制备了耗尽型的共漏极反向串联单片集成结构双向开关MOSFET器件,器件采用100nm厚度的Al<sub>2</sub>O<sub>3</sub>介质作为栅介质和钝化层。器件开关比高达10<sup>9</sup>,阈值电压为52.8V。通过短接两个栅极,器件为双向开关工作模式,当偏置电压大于阈值电压时可实现双向电流流动,在双向导通工作模式下分别实现了最大输出电流为180.52mA/mm、170.90mA/mm,导通电阻分别为0.20kΩ·mm、0.23kΩ·mm。双向开关器件的栅漏击穿电压在两个栅电极分别与相邻源电极短路时分别为-358V和366V,击穿场强约为0.22MV/cm,本研究为氢终端金刚石功率器件提供了新的应用示范场景。