Skip to content

Nanoscale NV-Center Magnetometry of a Synthetic Three-Dimensional Spin Texture

FieldValue
JournalThe Journal of Physical Chemistry C
Published2026-03-10
AuthorsRicardo Javier Peña Román, Sandip Maity, Fabian Samad, Dinesh Pinto, S. Josephy
DOI10.1021/acs.jpcc.6c00518

Quantitative NV-SPM mapped a surface stray field of approximately ±8.0 mT at antiferromagnetic domain boundaries. A (111)-oriented single-NV probe resolved approximately 100 nm-wide ferromagnetic stripes and 0 to 40 nm lateral domain-wall shifts. Local T1 relaxometry also detected magnetic noise consistent with the GHz range under ambient conditions.

The stack was [[Co(0.55 nm)/Pt(0.70 nm)]5/Co(0.55 nm)/Ru(0.75 nm)]3/[Co(0.55 nm)/Pt(0.70 nm)]6. Four ferromagnetic blocks have perpendicular magnetic anisotropy and are antiferromagnetically coupled through 0.75 nm Ru. Each block has a magnetic thickness of 6.8 nm, comparable to the 36 to 76 nm NV-sample distance.

Room-temperature dc magnetron sputtering used a base pressure of 8 × 10^-6 Pa and Ar at 0.4 Pa. The stack used silicon with 100 nm SiO2, a 1.5 nm Ta adhesion layer, a 20 nm Pt seed layer, and a 3 nm Pt oxidation cap.

SQUID-VSM measured an average saturation magnetization of (833 ± 83) kA/m for fully up or down configurations. Its four discrete hysteresis steps correspond to reversal of one ferromagnetic block at a time.

MeasurementReported condition
NV-sample distance36 to 76 nm
Probe orientations(100), (110), and (111)
Optical readout515 nm initialization; 650 to 850 nm photoluminescence collection
DC field sensitivityApproximately 2 µT/√Hz
ODMR map sampling3.5 nm pixels; 100 ms per pixel
MFM comparison15 nm tip-sample lift distance

All NV-SPM images used noncontact amplitude modulation.

Probe orientation separates spin mixing from noise

Section titled “Probe orientation separates spin mixing from noise”

With the (100)-oriented probe, the NV-axis angles were (113°, 270°) in the laboratory frame. Photoluminescence was quenched by about 40% along the ferromagnetic stripes. Local ODMR showed asymmetric splitting and less than 10% contrast at 2.80 GHz. The authors identified these features as evidence for several mT of off-axis stray field and spin mixing. Some stripe positions produced fields too strong for ODMR.

Previous NV-SPM studies of ultrathin systems involved magnetic thickness below 2 nm and only a few mT of stray field. An external field of 20 mT, applied 103° from the NV-axis, produced MFM-like contrast through field compensation. The model gave 23% contrast at 20 mT and 7% at 60 mT. The zero-field map returned after the external field was removed.

The (111)-oriented probe aligned the NV-axis with the out-of-plane magnetization. Its ODMR splitting stayed symmetric on both domains and stripes, which ruled out spin mixing as the quenching cause. The authors assigned the stripe quenching to magnetic noise.

MFM after in-plane saturation showed micrometer-scale antiferromagnetic domains separated by approximately 100 nm-wide ferromagnetic stripes. The average contrast period was approximately 300 nm.

The (111)-NV probe measured 0.6 mT on an antiferromagnetic domain and 4.0 mT on a stripe, projected onto the NV-axis. Dual iso-B maps found contours at -4.6 mT and +6.1 mT. A zero-field line marked the out-of-plane field sign reversal inside each stripe.

Reverse Fourier propagation reconstructed the two in-plane components from the measured out-of-plane component. The maximum static stray field was approximately ±8.0 mT at domain boundaries. Within the antiferromagnetic domains, in-plane and out-of-plane components ranged from hundreds of µT to 1 mT.

Granular contrast remained visible in the maps. The authors associated this granularity with local film nonuniformity and incomplete magnetization compensation.

The authors defined the domain wall as the line where the out-of-plane field changes sign. At 75 nm sensor height, the simulated zero-field line shifted several tens of nanometers toward the antiferromagnetic domain.

For a boundary between a ferromagnetic and an antiferromagnetic domain, the zero-field line differed from the line with zero out-of-plane magnetization. The extended stray field caused this difference. Measured profiles were asymmetric because the sensor sampled the top block and the full multilayer response. An analytical thin-sample fit was invalid because the magnetic thickness was comparable to the sensor distance.

Simulations reproduced alternating left and right wall shifts between adjacent ferromagnetic blocks. These shifts aligned moments through the stack and produced the reported three-dimensional texture. Measured shifts ranged from approximately 0 to 40 nm along the stripes.

Each block contained six Co layers separated by five Pt interlayers. Prior simulations of this architecture reported a constant shift of about 20 nm. The experiment instead found nonuniform shifts and ferromagnetic cores with different sizes and curved walls.

The (111) probe had a T1 of (1370 ± 142) µs with the tip withdrawn from the sample. T1 fell to (90 ± 9) µs over an antiferromagnetic domain and (14 ± 1) µs over a ferromagnetic stripe.

Probes with different crystallographic orientations showed essentially the same T1 change. This indicates noise components perpendicular to each NV-axis. The authors attributed the noise most likely to thermal magnons near the 2.87 GHz NV transition. This was an interpretation because the paper did not measure a direct spin-wave spectrum.

Stripe confinement was proposed to explain the shorter T1 over the stripe. It may provide stronger noise or a frequency closer to the NV electron spin resonance.

Lower laser power did not improve contrast, unlike the earlier model for antiferromagnetic walls. The local ferromagnetic core field splits the NV ms=±1 states and changes the initial conditions assumed by that two-level model.

Model agreement, limits, and device implications

Section titled “Model agreement, limits, and device implications”

The Mumax3 model used four 6.75 nm blocks separated by 0.75 nm Ru spacers. It used a 4 nm lateral cell within a 2.048 µm × 2.048 µm volume. The simulation volume extended 75 nm above the surface.

Simulated stray fields reached approximately ±12 mT, above the measured ±8.0 mT. The authors said magnetic parameters and the sensor distance required further optimization. The model reproduced the field-map pattern, granularity, wall shifts, and ferromagnetic cores.

A 2 nm mesh resolved more small-scale variation without changing the overall texture. It increased memory use and computation time, so the authors used 4 nm cells. Second-order anisotropy terms and interfacial DMI were omitted from the model.

Prior simulations of multilayered structures predict Néel-type walls in the outer blocks and Bloch-type walls in the middle. The present study did not directly determine the wall type. Refined micromagnetic simulations or Lorentz transmission electron microscopy were proposed for that task.

Varying sensor distance from 36 to 75 nm changed the extracted wall position by about 3 nm. This equaled about 8% of the distance span and depended on the selected profile.

Probe orientation is a material-selection variable for NV magnetometry, not merely a setup detail. A (111) probe aligned with out-of-plane magnetization supports quantitative vector mapping of thick synthetic antiferromagnets. Strong off-axis fields can quench photoluminescence and prevent ODMR at some stripe positions.

NV-SPM does not use the local MFM tip field, which can reach a few tens of mT and reorient magnetic moments. Device models should include nonuniform wall shifts, ferromagnetic cores, and GHz noise because these features affect local stray fields and relaxometry. Sensor distance and probe orientation should be reported with any nanoscale field measurement. The paper characterized magnetic texture rather than device operation or a direct spin-wave dispersion.

The experiment needs an oriented single-crystal diamond probe with one shallow NV center for quantitative magnetic imaging. The paper specifies a nominal 10 nm implantation depth and compares (100), (110), and (111) probe orientations. 6CCVD’s diamond materials catalog includes single-crystal MPCVD diamond, while the engineering support page can define requirements for the custom probe.

View Original Abstract

High Resolution Image Download MS PowerPoint Slide Multilayered synthetic antiferromagnets (SAFs) are artificial three-dimensional (3D) architectures engineered to create novel, complex, and stable spin textures. Noninvasive and quantitative nanoscale magnetic imaging of the two-dimensional stray field profile at the sample surface is essential for understanding the fundamental properties of the spin-structure and being able to tailor them to achieve new functionalities. However, the deterministic detection of spin textures and their quantitative characterization at the nanoscale remain challenging. Here, we use nitrogen-vacancy scanning probe microscopy (NV-SPM) under ambient conditions to perform the first quantitative vector-field magnetometry measurements in the multilayered SAF [(Co/Pt) 5 /Co/Ru] 3 /(Co/Pt) 6 . We investigate the static and dynamic nanoscale properties of antiferromagnetic domains with boundaries hosting “one-dimensional” ferromagnetic stripes with ∼100 nm of width and periodic modulation of the magnetization. By employing NV-SPM measurements in different imaging modes and involving NV-probes with various crystallographic orientations, we demonstrate distinct fingerprints emerging from GHz-range spin noise and constant stray fields on the order of several mT. This provides quantitative insights into the structure of domains and domain walls, as well as, into magnetic noise associated with thermal spin-waves. Our work opens up new opportunities for quantitative vector-field magnetometry of modern magnetic materials with tailored 3D spin textures and stray field profiles, and potentially novel spin-wave dispersions─in a quantitative and noninvasive manner, with exceptional magnetic sensitivity and nanometer scale spatial resolution.