Skip to content

Probing the Meissner effect in single crystals of Bi2Sr2Ca2Cu3O10+δ via wide-field quantum microscopy under high pressure

FieldValue
JournalApplied Physics Letters
Published2026-05-25
AuthorsM. Ohkuma, Ryo Matsumoto, Shintaro Adachi, Shinobu Onoda, Takao Watanabe
DOI10.1063/5.0334017

A local diamagnetic response in optimally doped Bi2Sr2Ca2Cu3O10+δ (Bi-2223) remained detectable at 23 GPa and 76±3 K when KBr transmitted the pressure. The response was suppressed above 11 GPa and 70 K when cBN served as the medium. Wide-field magnetometry based on nitrogen-vacancy centers in a diamond anvil produced this comparison without electrical contacts on the cuprate. The results show that the pressure environment can control the observed superconducting response of Bi-2223.

Pressure medium controls the observed transition

Section titled “Pressure medium controls the observed transition”

The ambient sample had a superconducting transition temperature, Tc, of about 110 K after oxygen annealing. The local response near 70 K at 23 GPa showed that screening persisted, although its reduced amplitude indicated a lower transition temperature under KBr. The cBN result showed a different outcome. Both media were solids, but they produced different levels of hydrostaticity.

Diamond anvil served as pressure window and magnetic sensor

Section titled “Diamond anvil served as pressure window and magnetic sensor”

The experiment used a type Ib diamond anvil with a 300 µm culet diameter and a (111)-oriented culet surface. The diamond provided the pressure window and hosted a thin NV layer at the sample interface. Wide-field imaging then resolved the local magnetic field at the cuprate position.

Local NV imaging avoids the sample-volume limit of bulk magnetometry and the contact and wiring burden of transport measurements. It can therefore image a Meissner response in a micrometer-sized sample without attaching electrodes to the cuprate.

The authors formed the NV centers by implanting 12C+ ions at 30 keV with a dose of 5 × 10^12 cm⁻². They annealed the anvil in vacuum at 1000 °C for 2 h. These details specify the sensor used for every reported comparison. No comparison of diamond grades or implantation doses was performed.

A CuBe diamond anvil cell contained the sensor and sample. The authors pre-indented a rhenium gasket to 50 µm and drilled a 250 µm hole. A cBN-epoxy mixture filled this hole and prevented contact between the microwave waveguide and the gasket. After pre-indentation, they drilled a 100 µm sample chamber.

A 5 µm Pt foil and the Bi-2223 single crystal were placed on the anvil. The chamber was filled with either cBN or KBr powder. Pressure was estimated from the diamond Raman shift at room temperature. The crystal was grown by the traveling-solvent floating-zone method and annealed at 500 °C under flowing 100% oxygen gas. The oxygen partial pressure was 1 atm.

The measurement cooled the cell below 20 K and began with zero-field cooling. Data were then acquired during warming. A magnetic field of about 4 mT was applied along the ⟨111⟩ direction. Below Tc, flux expulsion reduced the field sensed by NV centers beneath the cuprate. This Meissner response made the ODMR splitting over the sample smaller than the background splitting.

At 23 GPa and 76±3 K in KBr, three ODMR peaks were resolved. Two outer peaks came from field-aligned NV centers, while the central feature came from other orientations. Each spectrum took up to 15 min. The cold head was disabled during acquisition, so temperature increased during each scan. The reported temperature was the mean before and after acquisition, with the full interval used as uncertainty.

The analysis excluded points when the half-width of the 95% confidence interval for the fitted outer resonances exceeded 5 MHz. Regions with barely visible ODMR features were also excluded. The authors linked reduced visibility to weak microwave driving and insufficient signal-to-noise from limited averaging.

KBr gave clear diamagnetic signals below 80 K at 0, 6, and 11 GPa. The signal weakened as pressure rose, which the authors associated with a decreasing Tc. At 23 GPa, reduced ODMR splitting above the sample remained visible at 76±3 K. At the same pressure, the diamagnetic signal was absent at 124±3 K.

Persistence did not mean stabilization. The ambient Tc was about 110 K, while the KBr response persisted near 70 K under 23 GPa. The paper therefore supports retention of a detectable superconducting response under KBr, not a pressure-driven increase above the ambient Tc.

cBN caused suppression and partial recovery

Section titled “cBN caused suppression and partial recovery”

At 0 GPa, cBN produced a diamagnetic signal across the entire sample area. After pressurization, analyzable ODMR spectra came mainly from near the Pt foil. The authors detected a signal beneath the foil at 6 GPa. At 11 GPa, it was visible below the transition near 70 K, but no clear signal was found above 70 K.

At 19 GPa, no clear diamagnetic signal was detected down to 30 K with the setup. After pressure release from 19 GPa, a weak signal reappeared below 60 K. It occurred at a lower temperature than initially and its magnitude did not fully recover.

A missing local signal does not prove an insulating state or the absence of bulk superconductivity. The authors describe the behavior as consistent with strong suppression and a possible insulating-like evolution. They suggest that lattice distortion or grain refinement plays a significant role in the incomplete recovery, so compression alone does not explain it.

The result agrees with prior pressure-medium studies

Section titled “The result agrees with prior pressure-medium studies”

Earlier studies reported different Bi-2223 responses at high pressure. Fluid media produced an upturn in Tc, while solid media produced insulating-like transitions and loss of the zero-resistance state. The present cBN observations agree with earlier electrical results that found a much lower zero-resistance temperature and insulating-like resistance under cBN.

The same sensitivity appears in Bi-2212. cBN produced insulating-like behavior, while silicone oil produced a Tc increase above approximately 40 GPa. A NaCl-medium study found no obvious cracks and recovered zero resistance and metallic conductivity after pressure release. That recovery differs from the partial recovery observed here with cBN.

Hydrostatic conditions also matter in earlier comparisons. Hg-based cuprates reached zero resistance to approximately 22 GPa in a cubic anvil cell under hydrostatic pressure. SQUID measurements found the largest Tc under hydrostatic pressure compared with uniaxial strain. The current result adds a local magnetic observation. It does not equate a local diamagnetic signal with zero resistance.

Measurement limits and unresolved mechanisms

Section titled “Measurement limits and unresolved mechanisms”

Under pressure, the analyzable ODMR signal was concentrated near the Pt foil. The method sampled part of the cuprate rather than the full specimen. The nondetection down to 30 K at 19 GPa limits what the setup can resolve. It cannot establish that Tc fell below 30 K.

Temperature increased during each acquisition, although the reported uncertainty covered the full before-and-after interval. Pressure came from a room-temperature Raman measurement, not a low-temperature calibration. This study reported neither transport nor structural measurements alongside ODMR.

The authors call for systematic media comparisons, including fluid media inside the DAC. They also propose stress mapping and low-temperature pressure calibration to separate hydrostatic stress from non-hydrostatic stress and local strain. Quantum noise spectroscopy could provide further information if it can operate under high pressure. The mechanism behind the different cBN and KBr outcomes remains unresolved.

The work gives a concrete diamond design point for high-pressure NV magnetometry: a type Ib anvil with a 300 µm culet and a (111)-oriented surface. The NV layer was formed by 30 keV 12C+ implantation at 5 × 10^12 cm⁻², followed by 1000 °C vacuum annealing for 2 h.

The experiment supports integrating NV sensing with the diamond pressure window instead of relying on a separate bulk magnetometer. It also keeps transport contacts off the cuprate. The pressure medium remains a process variable because KBr and cBN produced different responses within the same measurement architecture. The study did not compare alternative diamond types, so the type Ib anvil is a reported implementation, not a proven optimum.

For this NV pressure-cell design, pressure-medium calibration belongs beside the diamond and NV specification.

View Original Abstract

We investigated the pressure dependence of the superconducting transition temperature (Tc) in optimally doped Bi2Sr2Ca2Cu3O10+δ (Bi-2223) single crystals using different pressure-transmitting media. Previous high-pressure studies have reported conflicting behaviors, ranging from a resurgence of Tc of optimally doped Bi-2223 in fluid media to an insulating-like transition in solid media. However, a direct comparison of the effects of different pressure-transmitting media is lacking. Here, we employed wide-field quantum microscopy based on nitrogen-vacancy centers to probe the magnetic response under high pressure, utilizing cBN and KBr as media. We observed that a diamagnetic response near 70 K, indicative of the superconducting transition, persisted up to 23 GPa in KBr, whereas it disappeared above 11 GPa and 70 K in cBN. These results demonstrate the high sensitivity of Bi-2223 to the pressure environment and highlight the critical role of hydrostatic pressure in cuprate superconductors.

  1. 2005 - Pressure-induced superconductivity in elemental materials [Crossref]
  2. 2010 - Silicon clathrates and carbon analogs: High pressure synthesis, structure, and superconductivity [Crossref]
  3. 2018 - Solids, liquids, and gases under high pressure [Crossref]
  4. 2023 - Signatures of superconductivity near 80 K in a nickelate under high pressure [Crossref]
  5. 2024 - Theoretical analysis on the possibility of superconductivity in the trilayer Ruddlesden-Popper nickelate La4Ni3O10 under pressure and its experimental examination: Comparison with La3Ni2O7 [Crossref]
  6. 2024 - Pressure-induced superconductivity in polycrystalline La3Ni2O7−δ [Crossref]
  7. 2024 - High-temperature superconductivity with zero resistance and strange-metal behaviour in La3Ni2O7−δ [Crossref]
  8. 2024 - Superconductivity in pressurized trilayer La4Ni3O10−δ single crystals [Crossref]
  9. 2004 - High-pressure phase diagram of Bi2Sr2CaCu2O8+δ single crystals [Crossref]
  10. 2010 - Enhancement of superconductivity by pressure-driven competition in electronic order [Crossref]