SOI wafer fabricated with a diamond BOX layer using surface activated bonding at room temperature
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-11-20 |
| Journal | Japanese Journal of Applied Physics |
| Authors | Yoshihiro Koga, Kazunari Kurita |
| Institutions | Sumco Corporation (Japan) |
| Citations | 4 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Novel SOI Architecture: A Silicon-On-Insulator (SOI) wafer is fabricated using a polycrystalline diamond buried oxide (BOX) layer, replacing the conventional thermally-limiting SiO2 BOX.
- Thermal Conductivity Improvement: The deposited diamond BOX layer demonstrated thermal conductivity approximately 3× higher than a conventional SiO2 layer, directly addressing self-heating issues in advanced semiconductor devices.
- Room-Temperature Bonding: A Surface-Activated Bonding (SAB) process at room temperature in ultrahigh vacuum (1 × 10-5 Pa) successfully bonded a silicon wafer to the diamond layer with zero detectable voids (>200 nm resolution).
- High-Temperature Resilience: The diamond-BOX SOI wafer maintained structural integrity through a 1000 °C device fabrication process, confirming suitability for next-generation power and high-frequency electronics.
- Damaging-Free Seeding: A non-destructive spin-coating technique using <10 nm nanodiamonds was utilized to seed the silicon base wafer, achieving a 28% surface nucleation density without surface damage.
- Polycrystalline Diamond Growth: Microwave Plasma-Enhanced CVD (MW-CVD) produced a dense 10 µm diamond layer (polished to 8 µm), confirmed by XRD to be polycrystalline with dominant (111) and (220) orientations.
- Application Targets: Designed specifically for self-heating-prone devices, including wireless communication components (5G/smartphones), automotive power electronics, and HD multimedia interfaces.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Base Wafer Material | Silicon (Si) | — | Substrate for diamond deposition |
| Seeding Method | Spin-coated nanodiamonds | — | < 10 nm grain size in water |
| Diamond Layer (As-Deposited) | 10 | µm | Thickness on 2-inch base wafer |
| Diamond Layer (Post-CMP) | 8 | µm | Thickness after polishing |
| Surface Roughness (Ra) | 2-3 | nm | Measured over 400 µm2 via AFM |
| Deposition Method | MW-CVD | — | Microwave Plasma-Enhanced CVD |
| Dominant Crystal Phases | (111), (220) | — | Polycrystalline diamond confirmed via XRD |
| sp3 Content | 285.4 | eV | Binding energy (XPS), indicating high-quality diamond |
| Bonding Method | SAB (Surface-Activated Bonding) | — | Room temperature process |
| Vacuum Level for Bonding | 1 × 10-5 Pa | — | Ultrahigh vacuum (UHV) chamber |
| Bonding Temperature | 25 (Room Temp) | °C | Avoids thermal stress and impurity diffusion |
| Voids at Interface | < 200 | nm | IR transmission, OM, and TEM confirmed void-free |
| Device Fabrication Temp | 1000 | °C | Subsequent annealing in N2 (2 hours) |
| BOX Thermal Conductivity | 3× SiO2 | — | Measured via TCi Thermal Property Analyzer |
| Contact Annealing | 900 (0.5h, N2) | °C | Post-implantation activation |
| Sintering Temp | 400 (0.5h, N2) | °C | Final metallization step |
Key Methodologies
Section titled “Key Methodologies”- Base Wafer Preparation: A 2-inch silicon wafer is cleaned and spin-coated with a water-based solution of <10 nm nanodiamonds.
- Seeding Activation: The wafer is baked to establish a uniform nucleation layer (28% surface coverage) characterized by XPS to confirm C-O/Si-O bonding (no direct C-Si bonds formed initially).
- Diamond Deposition (MW-CVD): A polycrystalline diamond layer is grown to 10 µm thickness using a methane/hydrogen plasma chemistry.
- Surface Polishing (CMP): Chemical Mechanical Polishing reduces the diamond layer to 8 µm and achieves an Ra of 2-3 nm suitable for SAB.
- Surface Activation: Both the diamond-coated base wafer and the bonding silicon wafer are irradiated with an Argon (Ar) ion beam to remove native oxides and create dangling bonds (sputter-cleaning).
- Room-Temperature Bonding (SAB): The wafers are brought into contact in a UHV chamber (1 × 10-5 Pa). C-Si bonds form at the interface without thermal annealing.
- Wafer Thinning: The top silicon wafer is ground and polished down to the desired device layer thickness.
- Device Fabrication: Standard CMOS-compatible processes are used, culminating in a 1000 °C anneal to test thermal stability.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”This research demonstrates a sophisticated application of polycrystalline diamond as a heat-spreading dielectric. Reproducing or extending this work requires highly uniform, ultra-smooth diamond films. Here is how 6CCVD supports this class of thermal management and semiconductor R&D:
- Applicable Materials: This paper specifically relies on a Polycrystalline Diamond (PCD) film. 6CCVD’s Optical Grade and Standard PCD plates (manufacturable up to 125 mm diameter, thicknesses 0.1 µm to 500 µm) are ideal candidates. The 8 µm-10 µm target thickness in the paper falls well within our standard deposition range. For applications demanding higher thermal conductivity, our Boron-Doped PCD offers tailored thermal and electrical properties.
- Customization Potential: The paper emphasizes the critical need for an Ra < 5 nm surface finish for successful room-temperature wafer bonding. 6CCVD provides in-house polishing achieving Ra < 5 nm on inch-size PCD wafers, directly satisfying this requirement. Furthermore, for devices requiring patterned electrodes or isolated thermal vias, our internal laser cutting and custom metalization services (Ti, Pt, Au, W, Cu) allow for the rapid prototyping of metallized diamond-on-silicon stacks.
- Engineering Support: Transitioning from a successful lab-scale SAB process to robust device manufacturing requires precise control over diamond morphology and stress. Our in-house PhD engineering team can consult on material selection, optimizing the sp3/sp2 ratio, and matching thermal expansion coefficients for SOI and high-frequency/power device integration.
- Logistics & Scale: Whether you need 2-inch R&D wafers (as used in this study) or are scaling toward 100 mm / 125 mm substrates, 6CCVD offers global shipping (DDU default, DDP available) to keep your development cycle moving without interruption.
For custom specifications, material consultation, or a quote on metalized diamond stacks, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We propose a fabrication process for a silicon on insulator (SOI) wafer with a diamond buried oxide (BOX) layer by combining nanodiamond-seeding deposition and a surface-activated bonding technique for high-frequency and power device applications. The diamond layer was deposited on a base wafer by the spin-coating of nanodiamonds and microwave-plasma-enhanced chemical vapor deposition. The thermal conductivity of this deposited diamond layer was three times that of a conventional SiO 2 layer. A silicon wafer was then bonded to the diamond layer at room temperature in ultrahigh vacuum without forming any voids. Additionally, this SOI wafer was used to fabricate devices at 1000 °C. Therefore, we believe that this SOI wafer with a diamond BOX layer and its fabrication process are important for the realization of self-heating devices such as next-generation high-frequency and power devices.