Fabrication of high thermal conductivity Cu/diamond composites at ambient temperature and pressure
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2019-08-01 |
| Journal | AIP Advances |
| Authors | Susumu Arai, Miyoka Ueda |
| Institutions | Shinshu University |
| Citations | 22 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Achievement: Fabrication of high thermal conductivity Cu/diamond composites reaching 662 W K-1 m-1, a 1.6x enhancement over pure Cu (~400 W K-1 m-1).
- Process Innovation: Electrodeposition technique conducted at ambient temperature and atmospheric pressure, eliminating the need for high-temperature/pressure sintering or infiltration.
- Material Used: Commercially available Single Crystal Diamond (SCD) particles in four grades (10 µm, 25 µm, 45 µm, and 230 µm).
- Optimal Particle Size: The composite with 230 µm diameter SCD particles at 61 vol.% loading delivered the highest thermal conductivity.
- Interface Quality: Dense microstructures with no observable gaps between Cu matrix and diamond particles, validated through FE-SEM cross-sectional analysis.
- Thermal Modeling: Experimental results closely matched Hasselman-Johnson theoretical predictions, confirming robust thermal interface conductance (~8.86×108 W m-2 K-1).
- Target Application: Heat dissipation components and heat sinks for high-power electronics and thermal management systems.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond particle sizes | 10, 25, 45, 230 | µm | MMP/SXD series (Changsha Xinye) |
| Optimal particle diameter | 230 | µm | Highest thermal conductivity result |
| Diamond volume fraction (peak) | 61 | vol.% | 230 µm particle composite |
| Peak thermal conductivity | 662 | W K-1 m-1 | Cu/diamond composite (230 µm) |
| Pure Cu thermal conductivity (reference) | ~400 | W K-1 m-1 | Electrodeposited pure Cu baseline |
| Diamond intrinsic thermal conductivity | 1300 | W K-1 m-1 | Assumed for modeling |
| Cu density | 8940 | kg m-3 | Used in property calculations |
| Diamond density | 3520 | kg m-3 | Used in property calculations |
| Cu specific heat capacity | 385 | J kg-1 K-1 | Used in property calculations |
| Diamond specific heat capacity | 512 | J kg-1 K-1 | Used in property calculations |
| Boundary conductance (assumed) | 8.86×108 | W m-2 K-1 | Cu/diamond interface |
| Plating bath | 0.85 M CuSO4·5H2O + 0.55 M H2SO4 | — | Aqueous electrolyte |
| Current density | 5 | mA cm-2 | Galvanostatic condition |
| Process temperature | Room temperature (~25) | °C | Ambient conditions |
| Process pressure | Atmospheric | — | Ambient conditions |
| Charge density (10/25/45/230 µm) | 54 / 135 / 243 / 1240 | C cm-2 | Fills ~2 particle layers |
| Thicker specimen charge density | 2500 | C cm-2 | 5.1 g of 230 µm particles |
| Diamond mass per layer (10/25/45/230 µm) | 0.11 / 0.28 / 0.50 / 2.53 | g | Single-cathode batch |
| Thermal diffusivity measurement | Xenon flash (LFA 447-2 Nanoflash) | — | Netzsch analyzer |
Key Methodologies
Section titled “Key Methodologies”- Raw Material Selection: Single crystal diamond particles (MMP series: 10, 25, 45 µm; SXD series: 230 µm) sourced as uncoated, granular powder.
- Electrolyte Preparation: Aqueous bath composed of 0.85 M CuSO4·5H2O and 0.55 H2SO4.
- Cell Architecture: Acrylic electrolytic cell (3.5 × 7 × 6 cm internal volume), horizontal electrode configuration with cathode at the bottom (3 × 6 cm exposed area).
- Electrode Configuration: Pure Cu plate as anode; stainless steel plate as cathode for composite deposition.
- Particle Precipitation: Diamond particles dispersed homogeneously in the bath via stir bar, then allowed to settle uniformly onto the cathode without aggregation.
- Electrodeposition: Galvanostatic Cu plating at 5 mA cm-2 to fill interstitial gaps between precipitated diamond particles.
- Charge Scaling: Total electrical charge scaled to particle size (54-1240 C cm-2) to ensure complete matrix infiltration.
- Specimen Recovery: Composites exfoliated from stainless steel cathode for characterization.
- Compositional Analysis: Diamond volume fraction quantified by weighing specimens after Cu matrix dissolution in HNO3.
- Microstructural Characterization: FE-SEM (Hitachi SU-8000) on cross-sections prepared by argon ion polishing (JEOL SM-09010).
- Thermal Measurement: Xenon flash diffusivity (Netzsch LFA 447-2) in thin-film mode for fine particles and bulk mode for 230 µm specimens.
- Theoretical Validation: Hasselman-Johnson model applied to predict thermal conductivity as a function of volume fraction and particle size.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”This research relies on clean, uncoated Single Crystal Diamond (SCD) particles in narrow size distributions across a wide range (10-230 µm). The 230 µm grade delivered the best thermal performance, suggesting that larger, high-purity SCD grains minimize phonon boundary scattering and maximize phonon transport across the Cu matrix interface.
| Paper Requirement | 6CCVD Match |
|---|---|
| High-purity SCD particles (10-230 µm) | Optical Grade SCD powders & grains, custom-screened to specification |
| Isotropic thermal conductivity | SCD substrates and crushed single crystals with controlled morphology |
| Clean surface (no metallic pre-coating) | Virgin, uncoated diamond—no Ti/Cr carbide-forming layers required |
Customization Potential
Section titled “Customization Potential”The study highlights that thermal conductivity scales strongly with particle size (10 µm → 230 µm produced a step-change in performance). For thermal management programs that require fine-tuning of grain size, volume fraction, or composite architecture:
- Custom Particle Grades: 6CCVD can provide SCD powders and granules tailored to size distributions beyond standard catalog offerings.
- Substrate & Wafer Forms: For researchers exploring alternative bonding routes (sintering, infiltration, brazing), PCD and SCD plates up to 125 mm diameter are available.
- Metalization for Hybrid Interfaces: If the deposition route is switched from electrolytic to brazed or sintered Cu/diamond, Ti, W, Cr, and Pt metallization are offered in-house to engineer robust carbide-forming interfaces—an alternative pathway to improve boundary conductance beyond the 8.86×108 W m-2 K-1 assumed in this paper.
- Laser Cutting & Dicing: Custom shapes and thicknesses (down to 0.1 µm for SCD freestanding films, up to 10 mm for substrates) for prototype heat spreader geometries.
- Boron-Doped Diamond (BDD): If active thermal-electrical coupling or integrated sensing/heat-spreading is desired in next-generation designs, BDD variants are available.
Engineering Support
Section titled “Engineering Support”This paper demonstrates that diamond-matrix interface engineering is the dominant lever for thermal composite performance. The authors achieved 1.6× pure Cu without any high-pressure sintering, validating the critical role of clean, uncoated diamond surfaces and proper wetting chemistry.
6CCVD’s in-house PhD engineering team can support similar thermal management composite development projects with:
- Material selection guidance (SCD vs. PCD vs. BDD, particle vs. wafer forms).
- Surface finish recommendations (Ra < 1 nm for SCD, < 5 nm for inch-size PCD).
- Metalization stack design for brazed or diffusion-bonded Cu/diamond architectures.
- Dimensional and tolerance consultation for custom heat sink geometries.
Call to Action
Section titled “Call to Action”For custom specifications, particle-size consultation, or material selection for next-generation thermal management composites, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
High thermal conductivity Cu/diamond composites were produced at ambient temperature and pressure using an electrodeposition technique, employing various diamond particle sizes in the range of 10 to 230 μm. The microstructures of the resulting composites were analyzed by scanning electron microscopy and their thermal conductivities were assessed using a Xenon flash instrument. The theoretical thermal conductivities of these materials were calculated based on the Hasselman-Johnson equation and compared with the experimentally determined values. The Cu/diamond composites produced in this work were found to exhibit compact textures without any gaps between the Cu matrix and the diamond particles, and the experimental thermal conductivities were in good agreement with the theoretical values. The specimen containing 61 vol.% of 230 μm diameter diamond particles had the highest conductivity of 662 W K-1 m-1, which is 1.6 times that of pure Cu (ca. 400 W K-1 m-1).