Characteristics of hydrogen-terminated single crystalline diamond field effect transistors with different surface orientations
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2020-01-01 |
| Journal | Acta Physica Sinica |
| Authors | Jinfeng Zhang, Jiamin Xu, Zeyang Ren, Qi He, Sheng-Rui Xu |
| Citations | 1 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Research Focus: Comparative analysis of hydrogen-terminated Single Crystal Diamond (SCD) Field Effect Transistors (FETs) fabricated on (110) and (111) crystal orientations, cut from a single 3.5 mm thick MPCVD-grown SCD bulk.
- Growth Method: Homoepitaxial MPCVD on High-Pressure High-Temperature (HPHT) diamond substrates, followed by laser cutting and mechanical polishing to isolate specific crystallographic planes.
- Key Device Achievement (111) Plane: Maximum saturation current of 80.41 mA/mm at VGS = -4 V, representing a ~1.4× improvement over the (110) plane device.
- Key Device Achievement (111) Plane: On-resistance of 48.51 Ω·mm, which is only 67% of the value observed for the (110) plane device.
- Carrier Transport Insights: Capacitance-Voltage (C-V) measurements indicate nearly identical maximum 2DHG hole concentrations ((110): 1.34 × 1013 cm-2; (111): 1.45 × 1013 cm-2), confirming that the (111) performance gain stems from lower sheet resistance rather than higher carrier density.
- Material Quality Validation: Raman and PL spectra confirm both (110) and (111) plates possess equivalent optical quality (Raman FWHM ≈ 3.9-4.0 cm-1), isolating surface orientation as the sole performance variable.
- Strategic Implication: Crystallographic orientation is a critical, tunable parameter for optimizing hydrogen-terminated diamond MESFETs targeting high-frequency and high-power RF applications.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Type | HPHT Diamond (Type Ib) | — | Homoepitaxial growth template |
| SCD Epitaxial Thickness | 3.5 | mm | Bulk growth for mechanical dicing |
| Crystal Orientations Tested | (110) and (111) | — | Cut from the same parent SCD bulk |
| Raman FWHM (1st order) | 3.9 - 4.0 | cm-1 | High crystalline quality indicator |
| Gate Length (Lg) | 6 | µm | MESFET architecture |
| Gate Width (Wg) | 50 | µm | MESFET architecture |
| Max Saturation Current IDS,max (110) | 58.02 | mA/mm | VGS = -4 V |
| Max Saturation Current IDS,max (111) | 80.41 | mA/mm | VGS = -4 V (1.4× higher) |
| On-Resistance Ron (110) | ~72.4 | Ω·mm | Estimated from 67% ratio |
| On-Resistance Ron (111) | 48.51 | Ω·mm | 67% of (110) device value |
| Max Transconductance gm (110) | 18.9 | mS/mm | Transfer characteristic metric |
| Max Transconductance gm (111) | 21.51 | mS/mm | Transfer characteristic metric |
| On/Off Ratio | ~108 | — | Normally-on depletion mode |
| 2DHG Concentration (110) | 1.34 × 1013 | cm-2 | Extracted from C-V |
| 2DHG Concentration (111) | 1.45 × 1013 | cm-2 | Extracted from C-V |
| Gate Leakage (110) | 4.0 × 10-4 | A/cm2 | At VGS = -4 V |
| Gate Leakage (111) | 1.4 × 10-4 | A/cm2 | At VGS = -4 V |
| Ohmic Contact Metal | Au (Gold) | — | 100 nm e-beam evaporated |
| Gate Metal | Al (Aluminum) | — | 100 nm e-beam evaporated |
| Schottky Barrier Height (Al/H-diamond) | 0.62 | eV | Reference value |
Key Methodologies
Section titled “Key Methodologies”- Substrate Pre-treatment: Sequential chemical processing — precision polishing, H2SO4/HNO3 (1:1) boiling at 250 °C for 1 hour to remove non-diamond carbon, followed by ultrasonic cleaning in acetone, ethanol, and DI water (15 min each).
- Damage Removal Etching: Hydrogen plasma treatment with 2% O2 for 30 minutes to eliminate polishing-induced mechanical subsurface damage.
- MPCVD Epitaxial Growth:
- Pressure: 320 mbar
- Substrate Temperature: 915 °C
- Microwave Power: 3.9 kW
- Total Gas Flow: 200 sccm
- CH4 Concentration: 6% in H2
- Crystal Orientation Isolation: Laser cutting and mechanical grinding/polishing of the 3.5 mm thick SCD wafer to produce individual (110) and (111) oriented plates from the same parent crystal.
- Hydrogen Termination: Hydrogen plasma treatment for 20 minutes, followed by cooling in pure H2 ambient to room temperature to form the C—H surface bonds required for 2DHG generation.
- Ohmic Contact Formation: E-beam evaporation of 100 nm Au, patterned via photolithography and KI/I2 wet etching; Au layer simultaneously protects the active channel H-termination.
- Device Isolation: Low-power oxygen plasma treatment for 10 minutes to convert H-terminated regions outside the active area into insulating O-terminated diamond.
- Gate Fabrication: E-beam evaporation of 100 nm Al with lift-off lithography, forming the Schottky gate contact.
- Characterization Suite: AFM for surface morphology, Raman spectroscopy (1st-order peak ~1332.5 cm-1) for crystalline quality, PL spectroscopy for optical defect analysis, and Keithley 4200 for I-V and C-V electrical characterization.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”-
Applicable Materials:
- This research fundamentally requires Optical/Electronic Grade Single Crystal Diamond (SCD) substrates and homoepitaxial layers. To replicate or extend this work, the following 6CCVD materials are directly applicable:
- Homoepitaxial SCD Wafers/Plates — grown via MPCVD on HPHT substrates, available in custom thicknesses up to 500 µm (with substrates extendable to 10 mm bulk for dicing operations such as those used in this paper).
- Surface-Oriented SCD Plates — 6CCVD can deliver SCD plates cut and polished to specific (100), (110), or (111) crystallographic orientations to support orientation-dependent device studies.
- Electronic Grade SCD — characterized by low nitrogen content and narrow Raman FWHM (< 2 cm-1 for premium grades), ideal for high-mobility 2DHG channel formation.
- This research fundamentally requires Optical/Electronic Grade Single Crystal Diamond (SCD) substrates and homoepitaxial layers. To replicate or extend this work, the following 6CCVD materials are directly applicable:
-
Customization Potential:
- Custom Metalization: The paper employs Au (100 nm) ohmic contacts and Al (100 nm) gate electrodes. 6CCVD offers in-house e-beam evaporation metalization with Au, Pt, Pd, Ti, W, and Cu — enabling tailored Schottky/ohmic stack engineering (e.g., Ti/Pt/Au for improved adhesion, or Au-only contacts as used here) without subcontracting delays.
- Laser Cutting & Dicing: 6CCVD provides precision laser cutting services for SCD and PCD materials, enabling researchers to obtain custom-shaped substrates from bulk crystals — directly supporting the workflow used to produce the (110) and (111) plates in this study.
- Custom Thickness: With SCD thickness range of 0.1 µm to 500 µm (and bulk substrates up to 10 mm), 6CCVD can supply both the thin epitaxial layers and thick bulk crystals required for dicing-based orientation studies.
- Surface Polishing: Ra < 1 nm polishing for SCD surfaces ensures minimal subsurface damage, complementing or replacing the O2/H2 plasma etching step used in this paper for damage removal.
-
Engineering Support:
- The orientation-dependent performance differences reported (1.4× IDS,max enhancement on (111) vs. (110)) suggest significant application-specific advantages. 6CCVD’s in-house PhD engineering team can assist with:
- Material selection between (100), (110), and (111) orientations for targeted MESFET, MOSFET, or 2DHG device architectures.
- MPCVD process optimization — recommending growth parameters (CH4/H2 ratios, pressure, temperature profiles) tailored to maximize 2DHG mobility and minimize sheet resistance for specific orientations.
- Metalization stack design for low-leakage Schottky gates and low-resistance ohmic contacts in hydrogen-terminated diamond FETs.
- Wafer geometry and dicing strategy consultation for researchers planning orientation-comparison studies from a single parent SCD crystal.
- The orientation-dependent performance differences reported (1.4× IDS,max enhancement on (111) vs. (110)) suggest significant application-specific advantages. 6CCVD’s in-house PhD engineering team can assist with:
-
Call to Action:
- For custom specifications, material consultation, or quotation on orientation-specific SCD substrates, custom metalization stacks, and precision-polished diamond plates, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Diamond has great potential applications in high-power, high-frequency semiconductor devices because of its wide band gap (5.5 eV), high thermal conductivity (22W/(cm·K)), and high carrier mobility (4500 cm<sup>2</sup>/(V·s) for electron, and 3800 cm<sup>2</sup>/(V·s) for hole). It has been widely considered as an ultimate semiconductor. From the analysis of our previous work, we find that the output current of field effect transistor based on hydrogen-terminated polycrystalline diamond is usually larger than that based on single crystal diamond, and that the preferential orientations of the polycrystalline diamond are mainly <inline-formula><tex-math id=“Z-20200108113531-1”>\begin{document}$ \langle 110\rangle $\end{document}</tex-math><alternatives><graphic xmlns:xlink=“http://www.w3.org/1999/xlink” xlink:href=“2-20191013_Z-20200108113531-1.jpg”/><graphic xmlns:xlink=“http://www.w3.org/1999/xlink” xlink:href=“2-20191013_Z-20200108113531-1.png”/></alternatives></inline-formula> and <inline-formula><tex-math id=“Z-20200108113531-2”>\begin{document}$ \langle 111\rangle $\end{document}</tex-math><alternatives><graphic xmlns:xlink=“http://www.w3.org/1999/xlink” xlink:href=“2-20191013_Z-20200108113531-2.jpg”/><graphic xmlns:xlink=“http://www.w3.org/1999/xlink” xlink:href=“2-20191013_Z-20200108113531-2.png”/></alternatives></inline-formula> shown by XRD results. Therefore, in order to further analyze the effect of surface orientation on the device performance of hydrogen-terminated diamond field effect transistor (FET), we study the devices fabricated respectively on the (110) plane and (111) plane single crystal diamond plates obtained from a single 3.5-mm-thick single crystal diamond grown by the microwave plasma chemical vapor deposition on the high-pressure high-temperature synthesized diamond substrate. Prior to processing the device, these diamond plates are characterized by atomic force microscope, Raman spectra and photoluminescence (PL) spectra. The results of Raman and PL spectra show that (110) plane and (111) plane plates originating from the same CVD single crystal diamond have no significant difference in optical property. Then the normally-on hydrogen-terminated diamond FET with a gate length of 6 μm is achieved. The device on (111) plane delivers a saturation drain current of 80.41 mA/mm at a gate voltage <i>V</i><sub>GS</sub> = -4 V, which is approximately 1.4 times that of the device on (110) plane. Meanwhile, the on-resistance of the device on (111) plane is 48.51 Ω·mm, and it is only 67% of the device on (110) plane. Analyses of the capacitance-voltage show that the hole concentration of the gated device on (110) plane and (111) plane are 1.34 × 10<sup>13</sup> cm<sup>-2</sup> and 1.45 × 10<sup>13</sup> cm<sup>-2</sup>, respectively, approximately at the same level. In addition, the hole density of the device on both (110) and (111) plane increase near-linearly with the increase of gate voltage from the threshold voltage to - 4 V, indicating that the control effect of the gate on the carrier in the channel is uniform. The possible reason for the higher saturation drain current as well as the lower on-resistance of the device on (111) plane is that its sheet resistance is lower.