Fabrication of AlGaAs/GaAs/diamond heterojunctions for diamond-collector HBTs
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2020-12-01 |
| Journal | AIP Advances |
| Authors | Sang June Cho, Dong Liu, Aaron Hardy, Jisoo Kim, Jiarui Gong |
| Institutions | Michigan State University, University of Wisconsin–Madison |
| Citations | 27 |
| Analysis | Full AI Review Included |
Technical Documentation: AlGaAs/GaAs/Diamond Heterojunction HBTs
Section titled “Technical Documentation: AlGaAs/GaAs/Diamond Heterojunction HBTs”Executive Summary
Section titled “Executive Summary”- Device Architecture: Demonstration of a novel p-n-p AlGaAs/GaAs/diamond Heterojunction Bipolar Transistor (HBT) to circumvent the lack of effective n-type dopants in diamond.
- Fabrication Method: A “grafting” technique was utilized to transfer an AlGaAs/GaAs membrane onto a single-crystalline p-type doped diamond substrate, forming a double-heterojunction.
- Material Properties: Single-crystalline p-type diamond with an exceptionally low electron affinity of 0.32 eV was integrated with conventional III-V semiconductors (AlGaAs/GaAs).
- Junction Performance: The AlGaAs/GaAs emitter-base p-n junction exhibited excellent rectification with an ideality factor of 1.09 and an Ion/Ioff ratio of 1.53 × 107 at ± 1.5 V.
- Collector Junction: The grafted GaAs/diamond n-p junction achieved a high Ion/Ioff ratio of 3.74 × 1010 at ± 5.2 V, despite a higher ideality factor of 3.67.
- Performance Limitation: A measured current gain slightly below unity (β < 1) was observed due to a 0.3 eV valence-band energy barrier between the GaAs base and the diamond collector.
- Future Outlook: Simulations indicate that further reducing the electron affinity of the p-type diamond could eliminate the base-collector barrier, enabling high current gain for next-generation high-power and RF applications.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond Bandgap (Eg) | 5.46 - 5.6 | eV | Ultrawide bandgap (UWBG) semiconductor property |
| Diamond Breakdown Field | ≥ 10 | MV/cm | High-power switching capability |
| Thermal Conductivity | > 2000 | W/m·K | Superior heat dissipation capability |
| Hole Mobility (µp) | 3800 | cm2·V-1·s-1 | High carrier mobility in diamond |
| Electron Mobility (µn) | 4500 | cm2·V-1·s-1 | High carrier mobility in diamond |
| Nitrogen Donor Level | ~1.7 | eV | Deep donor level limiting n-type doping |
| Phosphorous Donor Level | ~0.57 | eV | Deep donor level limiting n-type doping |
| Diamond Electron Affinity | 0.32 | eV | Critically low value for band alignment |
| AlGaAs Bandgap (Eg) | 1.8 | eV | Emitter layer bandgap |
| Al2O3 Bandgap | 3.75 (approx.) | eV | Passivation layer bandgap |
| GaAs Bandgap (Eg) | 1.42 | eV | Base layer bandgap |
| Valence Band Offset | 0.30 | eV | Energy barrier between GaAs base and diamond collector |
| Ideality Factor (Emitter-Base) | 1.09 | - | Near-ideal p-n junction behavior |
| Ion/Ioff (Emitter-Base) | 1.53 × 107 | - | Measured at ± 1.5 V |
| Ideality Factor (Base-Collector) | 3.67 | - | Grafted GaAs/diamond n-p junction |
| Ion/Ioff (Base-Collector) | 3.74 × 1010 | - | Measured at ± 5.2 V |
| GaAs Base Doping (n-type) | 6 × 1018 | cm-3 | Si-doped GaAs emitter contact layer thickness |
| Contact Layer Thickness | 40 | nm | n-GaAs top contact layer |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Utilization of single-crystalline p-type doped diamond (100) substrates.
- Epitaxial Growth: MOCVD/MBE growth of an AlGaAs(p-type)/GaAs(n-type) heterostructure membrane on a source wafer.
- Grafting Technique: Exfoliation and van der Waals bonding of the III-V membrane onto the p-type diamond substrate to form the base-collector junction.
- Surface Treatment: Chemical treatment and deposition of an Al2O3 passivation layer (3.75 eV bandgap) on the exposed diamond sidewalls to manage surface states and sidewall leakage.
- Contact Formation: Photolithography and metallization processes to define emitter, base, and collector contacts.
- Electrical Characterization: Measurement of diode characteristics (I-V curves) to extract ideality factors, rectification ratios, and HBT common-emitter current gain (β).
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”To replicate or extend this research, 6CCVD recommends the use of our high-purity Optical Grade Single Crystal Diamond (SCD). The device performance is fundamentally dependent on the diamond’s exceptionally low electron affinity (0.32 eV) to achieve proper band alignment with GaAs. Our SCD substrates are manufactured via MPCVD, ensuring the ultra-low defect density and precise p-type doping profiles required to suppress deep donor levels (like Nitrogen and Phosphorous) and minimize non-radiative recombination centers at the GaAs/diamond interface.
Customization Potential
Section titled “Customization Potential”The HBT architecture requires a precisely engineered GaAs/diamond n-p junction, which relies on a robust semiconductor-diamond bonding interface. 6CCVD offers comprehensive customization to support this:
- Custom Metalization: While the paper focuses on the active junction, any practical device requires robust ohmic contacts. 6CCVD provides internal metalization capabilities utilizing Ti, Pt, Au, Pd, W, and Cu to ensure low-resistance contact formation on both the III-V layers and the diamond collector.
- Laser Cutting & Shaping: To integrate the diamond collector into a functional HBT or module, 6CCVD offers precision laser cutting services. We can fabricate custom shapes and dimensions (up to 125mm for polycrystalline plates) to match specific device layouts.
- Thickness Control: Our SCD and PCD films can be fabricated in thicknesses ranging from 0.1µm to 500µm, allowing for optimized thermal management and reduced series resistance in the collector region.
Engineering Support
Section titled “Engineering Support”Navigating the complexities of band alignment between AlGaAs/GaAs and diamond—particularly minimizing the 0.3 eV valence band barrier—requires deep materials expertise. 6CCVD’s in-house PhD engineering team is available to assist with material selection, doping optimization, and wafer specifications for advanced high-power switching, RF, and heterojunction bipolar transistor projects. We work directly with research groups and commercial entities to tailor diamond material properties (such as polishing to Ra < 1nm for pristine epitaxial-ready surfaces) to meet exact experimental requirements.
Call to Action: For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Diamond is a highly attractive ultrawide bandgap semiconductor for next-generation high-power switching devices and RF devices for its superior physical and electrical properties. However, the lack of effective n-type dopants in diamond has limited the material to only unipolar p-type device applications. Heterostructure bipolar devices that use better n-type semiconductors together with p-type diamond is an approach to get high performance devices. In this work, p-n-p AlGaAs/GaAs/diamond heterojunction bipolar transistors (HBTs) are proposed and fabricated using a grafting technique. The double-heterojunction is formed by transferring an AlGaAs(p-type)/GaAs(n-type) membrane onto single-crystalline p-type doped diamond with an electron affinity of 0.32 eV. The epitaxial AlGaAs/GaAs emitter-base p-n junction shows an ideality factor of 1.09 with an Ion/Ioff of 1.53 × 107 at ± 1.5 V. The grafted GaAs/diamond n-p junction shows an ideality factor of 3.67 with an Ion/Ioff of 3.74 × 1010 at ± 5.2 V. Due to the valence-band energy barrier of 0.3 eV between the GaAs base and the diamond collector, the measured current gain for the HBT is slightly below unity. Simulations show that by reducing the electron affinity value of the p-type diamond, the base-collector energy barrier height can be correspondingly reduced, and high current gain can be expected.
Tech Support
Section titled “Tech Support”Original Source
Section titled “Original Source”References
Section titled “References”- 2005 - High Performance Devices World Scientific