DOUBLE-LAYER PLATES FROM SYNTHETIC DIAMOND SINGLE-CRYSTALS DOPED WITH NITROGEN FOR HIGH-TEMPERATURE n-TYPE SCHOTTKY DIODES
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2022-01-01 |
| Journal | IZVESTIYA VYSSHIKH UCHEBNYKH ZAVEDENIY KHIMIYA KHIMICHESKAYA TEKHNOLOGIYA |
| Authors | |
| Citations | 3 |
| Analysis | Full AI Review Included |
Double-Layer Nitrogen-Doped Diamond Plates for High-Temperature n-Type Schottky Diodes — Technical Documentation
Section titled “Double-Layer Nitrogen-Doped Diamond Plates for High-Temperature n-Type Schottky Diodes — Technical Documentation”Executive Summary
Section titled “Executive Summary”- Breakthrough Device Architecture: First fabricated and characterized vertical n-type Schottky diode based on a two-layer single-crystal diamond plate, where a thin lightly nitrogen-doped CVD layer is homoepitaxially grown on a heavily nitrogen-doped HPHT substrate.
- Active Doping Strategy: Uses nitrogen (N) as an alternative donor to phosphorus, eliminating the requirement for highly toxic phosphine (PH₃) gas during CVD growth, while delivering practical rectification at extreme temperatures.
- Electrical Performance: Turn-on voltage of approximately 30 V, forward current reaching 1 mA at U = 200 V, reverse leakage current below 0.1 µA (at T = 525-650 °C), and rectification ratio on the order of 104.
- Operating Regime: Stable current-voltage (I-V) characteristics verified across 525-650 °C, positioning diamond-based n-type diodes above the practical ceiling of current SiC-based high-temperature electronics (≈500 °C).
- Vertical Geometry: Uses Pt Schottky contact (200 nm) on the lightly-doped CVD epi-layer and a Ti/Pt (5 nm / 200 nm) ohmic contact on the HPHT substrate, with Au micro-wire bonding for characterization.
- Substrate Optimization Pathway: Identifies substrate thickness reduction (via ion-beam-assisted lift-off, down to ~1 µm) as the key enabler for reducing on-resistance from ~200 kΩ toward the ~1 Ω regime.
- Method: Combines TG-HPHT single-crystal substrate preparation with MPCVD homoepitaxial regrowth, opening a route to scalable nitrogen-doped n-type diamond electronics for high-temperature power and sensing.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate growth method | TG-HPHT (Temperature Gradient) | — | Single-crystal diamond substrate |
| HPHT growth pressure | 5.5 | GPa | C-Fe-Ni-Co growth system |
| HPHT growth temperature | 1500 | °C | Nitrogen adsorbed from ambient |
| Substrate orientation | {100} | — | Cut plate crystallographic plane |
| Substrate nitrogen concentration ([N] in C-centers) | ~200 ± 10 | ppm | By FTIR (1135 cm-1 peak, formula [13]) |
| Substrate thickness | 400 | µm | Reduced via lapping for I-V measurement |
| Substrate dimensions (pre-trim) | 8.0 × 4.0 × 0.4 | mm³ | Length × Width × Thickness |
| Final plate dimensions (post-trim) | 6.0 × 4.0 | mm² | After laser cutting of edges |
| Working layer growth method | Homoepitaxial MPCVD on {100} | — | Low-nitrogen regime in CH4/H2 |
| Epi-layer thickness (as-grown) | 50 | µm | Before back-thinning |
| Epi-layer thickness (final) | 10 | µm | After mechanical grinding/polishing |
| Epi-layer nitrogen concentration | ~0.5 | ppm | By UV absorption (270 nm peak, formula [17]) |
| Donor activation energy (N) | 1.7 | eV | Deep donor level in diamond |
| Boron acceptor reference (Ea) | 0.37 | eV | For context, p-type reference |
| Phosphorus donor reference (Ea) | ~0.6 | eV | For context, n-type reference |
| Substrate resistivity (500 °C) | 105 | Ω·cm | HPHT N-doped crystal |
| Substrate resistivity (650 °C) | 4 × 10³ | Ω·cm | HPHT N-doped crystal |
| Schottky contact metal | Platinum (Pt) | — | Magnetron sputtering via contact mask |
| Schottky Pt thickness | 200 | nm | Single-layer rectifying contact |
| Schottky contact diameter | 0.6 | mm | Six circular contacts per plate |
| Ohmic contact metal | Ti / Pt (TiC formed by anneal) | — | Magnetron sputtering via mask |
| Ohmic Ti thickness | 5 | nm | Pre-anneal deposition |
| Ohmic anneal temperature | 700 | °C | Vacuum anneal to form TiC |
| Ohmic Pt thickness (over Ti) | 200 | nm | Oxidation barrier for TiC |
| Ohmic contact shape | Rectangular (full back-side) | — | Single common backside contact |
| Wire bond material | Gold (Au) microwire, 40 µm | — | Ultrasonic compression bonding |
| Operating bias range | −200 to +200 | V | Full I-V characterization sweep |
| Tested temperature range | 525 to 650 | °C | High-temperature in-situ test |
| Test platform | Linkam TS1000 | — | Programmable thermal stage |
| Measurement instrument | Keithley 4200-SCS | — | Source-measurement unit |
| Turn-on voltage (Uon) | ~30 | V | Onset of strong forward conduction |
| Max forward current (single diode) | ~1 | mA | At U = 200 V |
| Reverse leakage current | < 0.1 | µA | At T = 525-650 °C |
| Rectification ratio | ~104 | — | On/off current ratio |
| On-resistance (Ron, measured) | ~200 | kΩ | Excess series (ballast) from thick substrate |
| On-resistance (target, thinned) | ~1 | Ω | Achievable via lift-off to ~1 µm |
| Step voltage (forward) | 65 - 85 | V | Current jumps ~1 order of magnitude |
| Linear I-V range | 150 - 200 | V | Fixed series-resistance regime |
| Resistivity temperature coefficient | ~5× decrease | — | 500 → 650 °C, series-resistance drop |
| IR absorption peak (C-centers) | 1135 | cm-1 | FTIR reference for [N] quantification |
| UV absorption peak (CVD epi) | 270 | nm | Used to compute 0.5 ppm [N] |
Key Methodologies
Section titled “Key Methodologies”-
HPHT Substrate Preparation
- Grow N-doped diamond single crystal via TG-HPHT at 5.5 GPa and 1500 °C in C-Fe-Ni-Co system, no nitrogen getter used (relies on ambient adsorption).
- Cut wafer in {100} plane (8.0 × 4.0 × 0.4 mm³), then mechanically polish.
- Quantify [N] via FTIR two-phonon reference band using formula from [13]:
N<sub>C</sub>[ppm] = 25 · α<sub>1135</sub>[cm<sup>-1</sup>], yielding ~200 ± 10 ppm.
-
Homoepitaxial CVD Regrowth
- Grow 50 µm of lightly N-doped diamond on the polished substrate via MPCVD with CH4/H2 chemistry (recipe detailed in ref [15]).
- Quantify [N] by UV absorbance at 270 nm (vs. IIa reference), using
N<sub>N</sub>[ppm] = 0.56 · α<sub>270</sub>[cm<sup>-1</sup>]→ ~0.5 ppm. - Laser-trim edges to 6.0 × 4.0 mm²; mechanically re-polish side facets.
-
Working-Layer Thinning
- Grind and polish the CVD layer from 50 µm down to 10 µm to define the active
n<sup>-</sup>working region. - Produces an
n<sup>+</sup>/n<sup>-</sup>two-layer single-crystal diamond stack ready for diode fabrication.
- Grind and polish the CVD layer from 50 µm down to 10 µm to define the active
-
Schottky Contact Formation
- Magnetron-sputter Pt (200 nm) through a shadow mask to define 6 circular Schottky contacts, each 0.6 mm Ø, on the lightly-doped CVD face.
-
Ohmic Contact Formation
- Magnetron-sputter Ti (5 nm) on the heavily-doped HPHT back-side, vacuum-anneal at 700 °C to convert Ti → TiC (carbide-forming ohmic).
- Sputter Pt (200 nm) over TiC to prevent atmospheric oxidation and serve as a Au-wire bond pad.
- Deposit a single rectangular (full-area) backside ohmic pad.
-
Assembly & Bonding
- Mount the diode plate in a Linkam TS1000 thermal stage.
- Ultrasonic compression-bond 40 µm Au microwires from each Schottky pad to external probes.
-
Electrical Characterization
- Sweep U = −200 V → +200 V with Keithley 4200-SCS while holding T at 525, 550, 575, 600, 625, 650 °C.
- Extract Uon, Imax, Irev, rectification ratio, and Ron(T) at each step.
-
Roadmap for Optimization (declared by authors)
- Reduce HPHT substrate thickness to ~1 µm via ion-beam-assisted lift-off (refs [1, 2]).
- Extend contact area across the wafer to lower Ron toward ~1 Ω.
- Investigate alternative Schottky metals (Al, Ni) per ref [19].
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”-
Applicable Materials
- Optical-Grade Single-Crystal Diamond (SCD), {100} orientation — required to replicate the HPHT substrate and homoepitaxial regrowth step. 6CCVD supplies {100} SCD substrates with controlled N-doping and FTIR/UV-verifiable nitrogen concentrations, plus MPCVD homoepitaxial layers from 0.1 µm to 500 µm.
- Nitrogen-Doped SCD Wafers — used as the heavily-doped HPHT-equivalent substrate. We provide thickness control from thin contact-ready foils up to 10 mm substrates, enabling either the 400 µm geometry or thinned versions needed to drop Ron.
- Optical-grade, Low-N MPCVD SCD layers — epitaxial regrowth layers with < 1 ppm substitutional nitrogen on demand, matching the 0.5 ppm epi-spec. Available in custom thicknesses down to single-micron tolerance.
- Heavy Boron-Doped PCD (BDD) is available as a complementary p-type reference for benchmarking and for parallel
p<sup>+</sup>/p<sup>-</sup>Schottky diode studies when comparing with literature [1, 2].
-
Customization Potential
- Plates / wafers up to 125 mm (PCD) and SCD substrates in custom footprints (the paper uses 6.0 × 4.0 mm²; 6CCVD routinely produces smaller and far larger geometries).
- Sub-micron thinning (lift-off / lapping & polishing): Routine SCD polishing to Ra < 1 nm; controlled back-thinning down to the ~1 µm regime needed to drop series resistance from ~200 kΩ toward the ~1 Ω theoretical target.
- Metallization (in-house): Ti, Pt, Pd, Au, W, Cu stacks including Ti/Pt/Au and TiC-forming ohmics with the 5 nm Ti + 200 nm Pt architecture used in this paper. Evaporation and magnetron sputtering through contact masks available as standard services.
- Schottky-metal flexibility: Pt shown here; we also support Au, Pd, and Cu overlays — and can co-deposit Al/Ni variants recommended by the authors for future diode-architecture studies.
- Laser cutting & die preparation: Edge trimming, contact-window opening, and side-facet polishing as described in the methodology, to deliver diode-ready plates.
-
Engineering Support
- Our in-house PhD engineering team can assist with vertical Schottky-diode stack design — including doping-profile selection (C-center nitrogen content, 0.5-500 ppm), epi-layer thickness optimization (sub-10 µm target to lower Uon), and metallization stack matching for high-temperature electronics (>500 °C), nuclear microbattery betavoltaics, and harsh-environment power rectification.
- We provide FTIR (1135 cm-1) and UV (270 nm) [N] quantification on every substrate/each growth run, ensuring traceability from raw boule to finished diode plate.
-
Call to Action
- For custom dimensions, controlled nitrogen doping, Ti/Pt ohmics, Pt Schottky metallization, or sub-µm SCD thinning for next-generation high-temperature Schottky diodes, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
For the first time, a vertical Schottky diamond diode with an electronic type of conductivity was manufactured and investigated on the basis of a two-layer single-crystal plate of synthetic diamond doped with nitrogen, in which a thin working layer of low-nitrogen-doped diamond was grown by the chemical vapor deposition method homoepitaxially on a heavily nitrogen-doped substrate cut in the plane {100} from a single crystal grown by the method of high-pressure-high-temperature growth on the seed. The concentration of nitrogen in the form of single substitution atoms (C-centers) in the working layer, grown by the chemical vapor deposition method, was 0.5 ppm, the layer thickness was 10 μm, the thickness of the substrate with a nitrogen concentration of ~ 200 ppm was 400 μm. 6 Schottky contacts with a diameter of 0.6 mm were made by magnetron sputtering of a platinum layer with a thickness of 200 nm through a contact mask. A rectangular ohmic contact was made to the substrate also by magnetron sputtering through a contact mask of a 5 nm thick Ti layer, followed by high-temperature annealing in vacuum to form titanium carbide, and subsequent deposition of a Pt layer with a thickness of 200 nm to prevent oxidation of titanium carbide in air. The current-voltage characteristics of the manufactured diodes were studied at a bias range of (-200 V) - (+200) V at temperatures up to 650 °C. The opening voltage of the manufactured diode structure is ~ 30 V, the maximum current of each diode in the open state reaches 1 mA at U = 200V, while the reverse current at T = 525-650 °C does not exceed 0.1 µA. The highest rectification coefficient value was ~104.