Comparison of thermal stabilities of p+-Si/p-diamond heterojunction and Al/p-diamond Schottky barrier diodes
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2022-04-05 |
| Journal | Japanese Journal of Applied Physics |
| Authors | Yota Uehigashi, Shinya Ohmagari, Hitoshi Umezawa, Hideaki Yamada, Jianbo Liang |
| Institutions | National Institute of Advanced Industrial Science and Technology, Osaka City University |
| Citations | 4 |
| Analysis | Full AI Review Included |
Comparison of Thermal Stabilities of p+-Si/p-Diamond Heterojunction and Al/p-Diamond Schottky Barrier Diodes
Section titled “Comparison of Thermal Stabilities of p+-Si/p-Diamond Heterojunction and Al/p-Diamond Schottky Barrier Diodes”Executive Summary
Section titled “Executive Summary”- Research Focus: Systematic evaluation of thermal stability in p+-Si/p-diamond heterojunction diodes (HDs) versus conventional Al/p-diamond Schottky barrier diodes (SBDs) under high-temperature annealing conditions.
- Fabrication Method: Surface-activated bonding (SAB) used to create Si/diamond heterojunctions, enabling direct comparison with Al/diamond SBDs on identical diamond substrates.
- Critical Finding: Si/diamond HDs maintain diode integrity up to 873 K (improved ideality factor, reverse-bias current, and on/off ratio), while Al/diamond SBDs show monotonic degradation due to Al3C4 carbide formation at 1020 K.
- Optimal Annealing Temperature: 873 K yields barrier height of 0.58 eV for Si/diamond HDs, closely matching the intrinsic S ≈ 1 correlation line for metal/diamond interfaces.
- Thermal Failure Mechanism: At 1073 K, HD characteristics degrade due to intermediate layer formation and thermal strain from CTE mismatch (Si/diamond Δα ≈ 1.8 × 10-6 °C-1).
- Application Impact: Si/diamond HDs demonstrate superior thermal robustness for aerospace, industrial processing, and high-temperature power electronics environments.
- Diamond Material Requirement: Lightly doped (2 × 1016 cm-3) B-doped drift layer epitaxially grown on heavily doped (~1020 cm-3) (100) diamond substrate with sub-nanometer surface roughness.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond Substrate Dopant (B) | ~1020 | cm-3 | Heavily doped (100) substrate |
| Drift Layer Dopant (B) | 2 × 1016 | cm-3 | Lightly doped epitaxial layer |
| Drift Layer Thickness (as-grown) | 25 | µm | Epitaxial CVD growth |
| Drift Layer Thickness (polished) | 21 | µm | Post-mechanical polishing |
| Diamond Surface Roughness (Ra) | 1.0 | nm | Post-polishing AFM measurement |
| Si Surface Roughness (Ra) | 0.1 | nm | SOI device layer |
| SOI Device Layer Thickness | 2.5 | µm | p+ B-doped (~1019 cm-3) |
| SOI Buried Oxide Thickness | 1 | µm | SiO2 layer |
| Diamond Bandgap | 5.5 | eV | Wide bandgap semiconductor |
| Diamond Breakdown Field | >10 | MV cm-1 | Power device capability |
| Hole Mobility | 3800 | cm2 V-1 s-1 | Intrinsic diamond property |
| Electron Mobility | 4500 | cm2 V-1 s-1 | Intrinsic diamond property |
| Dielectric Constant (εdia) | 5.7 | — | Relative permittivity |
| Effective Carrier Mass (m*) | 0.908 m0 | — | Used in TFE + BL model |
| Annealing Temperature Range | 703-1073 | K | Thermal stability evaluation |
| Critical Failure Temperature (Al SBD) | 1020 | K | Al3C4 carbide formation |
| Barrier Height (HD, unannealed) | 0.54 | eV | Richardson plot |
| Barrier Height (HD, 703 K annealed) | 0.93 | eV | Richardson plot |
| Barrier Height (HD, 873 K annealed) | 0.58 | eV | Richardson plot, near-intrinsic |
| Barrier Height (HD, 1073 K annealed) | 0.50 | eV | Richardson plot, degraded |
| Barrier Height (Al SBD, unannealed) | 0.91 | eV | Richardson plot |
| Barrier Height (Al SBD, 873 K annealed) | 0.31-0.53 | eV | TFE + BL model range |
| Barrier Height (Al SBD, 1073 K annealed) | 0.21 | eV | Severe degradation |
| CTE Mismatch (Si vs Diamond) | 1.8 × 10-6 | °C-1 | Thermal expansion difference |
| Hump Feature in I-V | ~-1.4 | V | Interface inhomogeneity indicator |
Key Methodologies
Section titled “Key Methodologies”- Diamond Epitaxial Growth: 25 µm lightly B-doped (2 × 1016 cm-3) drift layer grown via CVD on heavily B-doped (~1020 cm-3) (100) diamond substrate.
- SOI Preparation: Silicon-on-insulator substrate with 2.5 µm p+-Si device layer (~1019 cm-3 B-doped) on 1 µm SiO2/Si(100) handle wafer.
- Surface Polishing: Mechanical polishing of diamond drift layer surface to achieve Ra = 1.0 nm; final thickness 21 µm.
- Surface-Activated Bonding (SAB): Si device layer bonded to polished diamond surface under vacuum at room temperature using Ar beam activation.
- Substrate Removal: Si handle wafer and buried SiO2 removed via grinding and wet chemical etching to expose p+-Si/p-diamond heterojunction.
- Mesa Formation: p+-Si mesas defined by wet etching; ohmic contact (Ti/Au) deposited on diamond backside.
- Schottky Contact Fabrication: Al/Ni/Au Schottky contacts deposited on diamond for reference SBDs.
- Thermal Annealing Protocol: Sequential annealing at 703 K, 873 K, and 1073 K for durability evaluation.
- Electrical Characterization: Current-voltage (I-V) and temperature-dependent I-V measurements (Richardson plots) for barrier height extraction via thermionic emission (TE) and thermionic field emission + barrier lowering (TFE + BL) models.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”The research presented here demonstrates critical requirements for high-temperature diamond electronics that align directly with advanced material specifications achievable through custom manufacturing services.
Applicable Materials
Section titled “Applicable Materials”| Research Requirement | Solution |
|---|---|
| Heavily B-doped (100) diamond substrate (~1020 cm-3) | High-conductivity BDD substrates with controlled doping profiles |
| 25 µm epitaxial drift layer (2 × 1016 cm-3 B-doped) | Custom epitaxial CVD layers with precision boron concentration control |
| Sub-nm surface roughness (Ra 1.0 nm) | Ultra-precision polishing achieving Ra < 1 nm for SCD and < 5 nm for inch-size PCD |
| (100) crystallographic orientation | Orientation-controlled single-crystal and polycrystalline growth |
For replicating the heterojunction diode architecture, Optical Grade SCD wafers with controlled B-doping would serve as the substrate foundation. The epitaxial drift layer specifications (thickness, doping uniformity, surface finish) represent a custom growth service requiring precise CVD parameter control.
Customization Potential
Section titled “Customization Potential”The paper’s device structure necessitates several custom capabilities beyond standard catalog offerings:
- Custom Thickness Control: The 25 µm epitaxial drift layer (post-polishing 21 µm) falls within standard thickness capabilities (0.1 µm - 500 µm), but the precise doping gradient (heavy substrate → light epilayer) requires custom epitaxial reactor programming.
- Metalization Stack Replication: The device employs Ti/Au ohmic contacts on diamond and Al/Ni/Au Schottky contacts. Internal metalization capabilities support Au, Pt, Pd, Ti, W, and Cu depositions with custom layering sequences.
- Laser Cutting Services: Mesa formation and device isolation can be supported through precision laser dicing to achieve the lateral dimensions required for SAB-compatible bonding interfaces.
- Wafer Scaling: The 125mm PCD plate capability provides scalable substrate options for moving from research-scale demonstration to pilot production.
Engineering Support
Section titled “Engineering Support”The thermal stability comparison methodology—requiring identical diamond substrates for HD and SBD fabrication—underscores the value of working with a supplier who understands device-level integration challenges. The in-house PhD engineering team provides material consultation for projects involving:
- Si/diamond and III-N/diamond heterojunctions for power electronics thermal management
- High-temperature Schottky diode development using thermally robust contact metallization
- B-doping gradient engineering for drift layer optimization
- Surface preparation protocols for bonding-compatible diamond surfaces
The research explicitly notes that “the characteristics of Si/diamond HDs annealed at 873 K are close to their intrinsic properties” (barrier height 0.58 eV matching the S ≈ 1 correlation line). Achieving these intrinsic properties requires material with minimal defect density, precise epitaxial control, and exceptional surface finish—all of which depend on CVD growth expertise.
Call to Action
Section titled “Call to Action”For custom diamond substrates, epitaxial layers, metalization stacks, or material consultation for heterojunction power device research, visit 6ccvd.com or contact the engineering team directly.
View Original Abstract
Abstract We evaluate the current-voltage ( I-V ) and temperature-dependent I-V characteristics of p + -Si/p-diamond heterojunction diodes (HDs) fabricated using surface-activated bonding and compare their characteristics with those of Al/p-diamond Schottky barrier diodes (SBDs) fabricated on the same diamond substrate. The ideality factor, reverse-bias current, and on/off ratio of HDs are improved by annealing them at temperatures up to 873 K, which is in good contrast to the characteristics of SBDs. The barrier height at Si/diamond bonding interfaces is decreased by annealing. The difference in response to annealing between HDs and SBDs implies that the density of interface states formed during the surface activation process is decreased by annealing HDs. The characteristics of HDs are degraded by annealing them at 1073 K, which is assumed to be due to the formation of intermediate layers or the occurrence of local strain at Si/diamond bonding interfaces.