Local Ferromagnetic Resonance Measurements of Mesoscopically Patterned Ferromagnets Using Deterministically Placed Nanodiamonds
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2022-12-01 |
| Journal | Physical Review Applied |
| Authors | Jeffrey Rable, Benjamin Piazza, Jyotirmay Dwivedi, Nitin Samarth |
| Institutions | Pennsylvania State University |
| Citations | 4 |
| Analysis | Full AI Review Included |
Local FMR Measurements via Deterministic Nanodiamond Placement
Section titled “Local FMR Measurements via Deterministic Nanodiamond Placement”Executive Summary
Section titled “Executive Summary”- Core Innovation: Demonstration of an atomic force microscopy (AFM) “pick-and-place” technique to deterministically position nitrogen-vacancy (NV) nanodiamonds at targeted sites on patterned Permalloy (Py) thin-film structures with sub-100 nm placement accuracy.
- Methodology Achievements: Implementation of optically detected ferromagnetic resonance (ODFMR) measurements using 40-100 nm nanodiamonds on 5-10 µm mesoscopic Py features (10 nm thickness) to spatially resolve magnetization dynamics.
- Key Finding: Detection of distinct ferromagnetic resonance (FMR) signals at the bulk vs. edges of patterned features, revealing higher-order magnon modes and local distortions caused by fabrication defects (specifically near a constriction between two Py disks).
- Validation: Experimental results showed strong agreement with micromagnetic simulations using Mumax3 (saturation magnetization Ms = 8 x 105 A/m, exchange stiffness Aex = 1.3 x 10-11 J/m, Gilbert damping α = 0.0063).
- Optical Setup: A 1 mW, 532 nm continuous-wave laser was used for NV initialization and readout, with microwave excitation delivered via a 25 µm diameter gold wire across the sample.
- Application Scope: The methodology provides a more flexible alternative to scanning probe NV magnetometry or FMR force microscopy for probing local spin dynamics in magnonic devices, artificial spin ice, skyrmions, and domain walls.
- Significance: Offers new capabilities for characterizing spin wave edge modes and nanoscale magnetic textures without requiring sophisticated instrumentation or lithographic templating.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Nanodiamond size range | 40 - 100 | nm | Probe particle dimensions for deterministic placement |
| Placement accuracy | < 100 | nm | AFM-assisted positioning precision |
| Laser wavelength | 532 | nm | NV center optical excitation |
| Laser power | 1 | mW | Continuous-wave operation for fluorescence readout |
| Microwave wire diameter | 25 | µm | Gold wire for FMR and NV spin driving |
| Permalloy film thickness | 10 | nm | Thickness of patterned magnetic features |
| Feature lateral size | 5 - 10 | µm | Mesoscopic Py islands/disks |
| Disk diameter | 6 | µm | Circular Py features measured |
| Rectangular dimensions | 10 x 5 | µm | Rectangular Py island tested |
| NV sensor proximity | < 100 | nm | Required sample-probe separation for ODFMR sensitivity |
| Saturation magnetization (Ms) | 8 x 105 | A/m | Permalloy parameter for Mumax3 simulations |
| Exchange stiffness (Aex) | 1.3 x 10-11 | J/m | Micromagnetic simulation input |
| Gilbert damping (α) | 0.0063 | — | Permalloy damping parameter |
| Simulation cell size | 5 x 5 x 10 | nm | Mumax3 discretization |
| Gaussian pulse amplitude | 0.5 | mT | FMR excitation in simulations |
| Gaussian pulse FWHM | 20 | ps | Excitation temporal width |
| Simulation evolution time | 20 | ns | Time-domain propagation |
| Sampling interval | 5 | ps | Magnetization readout cadence |
| Frequency resolution | 50 | MHz | Discrete FFT output |
| Applied bias field range | 1 - 30 | mT | Range explored in simulations |
| Magnet type | N52 | — | Permanent magnet for static bias field |
| In-plane anisotropy field (B∥) | 3.3 | mT | Measured from Kittel equation fitting |
| Out-of-plane anisotropy field (B⊥) | 1.04 | T | Close to theoretical 1 T Ms of Py |
| Starting FMR frequency (easy axis) | ~2 | GHz | Minimum resonance at zero field |
| APD model | ID Quantique ID100 | — | Single-photon avalanche photodiode for readout |
| Simulation software | Mumax3 | — | GPU-accelerated micromagnetic solver |
Key Methodologies
Section titled “Key Methodologies”-
Substrate Preparation
- Drop-cast 40-100 nm NV-containing nanodiamonds onto a calibration substrate for AFM tip pickup.
- Patterned Py thin films (10 nm thickness) on separate substrates featuring rectangular islands (10 x 5 µm) and dual-disk geometries (6 µm diameter circles connected at edges).
-
AFM-Based Nanodiamond Pickup
- Scan substrate to identify nanodiamond particles matching dispersed sizes (Fig. 1, step 1).
- Engage ramp mode and ramp AFM tip into the particle.
- Re-scan area to confirm particle pickup by verifying absence (Fig. 1, step 2).
-
Deterministic Placement of Nanodiamonds
- With nanodiamond adhered to tip, scan target sample to locate feature of interest (Fig. 1, step 3).
- Deposit nanodiamond via either:
- Ramp-and-displace: Ramp tip into feature until particle dislodges.
- Lift-mode scraping: Maintain constant tip height below surface while scanning to release particle.
- Perform post-placement scan to confirm location on targeted site (Fig. 1, step 4).
- Repeat as needed to position multiple nanodiamonds at different locations on the same sample.
-
Optical Polarization and Readout
- Apply 1 mW, 532 nm CW laser through scanning mirror for NV initialization and fluorescence imaging.
- Collect fluorescence via ID Quantique ID100 avalanche photodiode (APD).
- Scan confocal fluorescence mapped onto AFM topography for co-registration.
-
Magnetic Field Calibration
- Apply static in-plane field via N52 permanent magnet on repeatable stepper motor linear stage.
- Calibrate using single-crystal diamond film with known NV orientations and Zeeman splitting.
-
ODFMR Measurement
- Drive FMR using 25 µm gold wire microwave delivery across the sample.
- Record NV fluorescence contrast as a function of applied magnetic field sweep (0-30 mT).
- Detect FMR-induced quenching of NV fluorescence attributed to enhanced magnon density and magnetic noise.
-
Micromagnetic Simulation (Mumax3)
- Discretize Py geometry into 5 x 5 x 10 nm cells.
- Initialize magnetization along (0,0,1) out-of-plane and relax to minimum energy under 1-30 mT bias.
- Apply 20 ps FWHM, 0.5 mT amplitude Gaussian pulse.
- Evolve Landau-Lifshitz-Gilbert equation for 20 ns with 5 ps sampling.
- Apply discrete FFT for frequency-domain analysis (50 MHz resolution).
-
Data Analysis
- Fit observed FMR dispersions to geometry-dependent Kittel equation for anisotropy extraction.
- Compare bulk vs. edge signals for detection of higher-order magnon modes and defect-induced distortions.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”The experiments rely on two complementary diamond material forms:
-
NV-Containing Nanodiamonds (40-100 nm): For probe particles, 6CCVD offers custom-sized nanodiamond powders with controlled NV center concentrations. These are suitable for drop-casting and deterministic placement protocols. Our nanodiamonds can be provided with specified size distributions and nitrogen content to ensure reliable T1/T2 performance for ODFMR sensitivity.
-
Single-Crystal Diamond (SCD) Film for Calibration: The paper used a single-crystal diamond film containing NV centers for in-plane magnetic field calibration via Zeeman splitting. 6CCVD’s Optical Grade SCD substrates and films (available in thicknesses from 0.1 µm to 500 µm, with polishing to Ra < 1 nm) are ideal for this calibration role. Custom (111)-oriented or (100)-oriented films can be supplied with controlled NV layer depth profiles.
Customization Potential
Section titled “Customization Potential”-
Dimensional Control: The Py features measured were on the order of 5-10 µm, well within the range of substrates 6CCVD can provide. Our polycrystalline diamond (PCD) substrates up to 125 mm and SCD up to 125mm accommodate both microscale device arrays and full wafer-scale integration.
-
Metalization for Microwave Delivery: The 25 µm gold wire used for microwave excitation was manually placed; researchers requiring integrated microwave structures (e.g., coplanar waveguides, striplines, or patterned antenna structures) can leverage 6CCVD’s internal metalization capabilities including Au, Pt, Pd, Ti, W, and Cu deposition. This allows hybrid integration of diamond sensors directly onto lithographically defined microwave circuits for improved ODFMR signal delivery.
-
Laser Cutting and Dicing: For experiments requiring custom-shaped diamond membranes or isolated sensor elements, 6CCVD provides laser cutting services to achieve precise geometries from stock substrates.
-
Thickness Engineering: Thin SCD films (down to 0.1 µm) are available for applications requiring minimal probe-sample separation, critical for ODFMR sensitivity (which decreases rapidly with distance).
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD engineering team has direct experience supporting spintronics and quantum sensing research programs. We can assist with:
- Material Selection: Recommending the optimal NV density and diamond form (SCD vs. PCD vs. nanodiamond) for your specific ODFMR or magnetometry experiment.
- Surface Preparation: Advising on surface termination (hydrogen, oxygen) and cleaning protocols to minimize fluorescence quenching when nanodiamonds are placed near metallic thin films.
- Co-Design for Pick-and-Place: Providing nanodiamonds with size distributions matched to your AFM tip geometry and placement protocol.
- Hybrid Integration: Coordinating diamond metalization patterns that are compatible with ferromagnetic thin-film deposition and lithographic processing.
Whether you are probing magnon edge modes, artificial spin ice arrays, single magnetic nanowires, or domain wall dynamics, 6CCVD can tailor diamond specifications to accelerate your research timeline.
Call to Action
Section titled “Call to Action”For custom specifications, bulk nanodiamond orders, metalized diamond substrates, or material consultation for your spintronics and NV-magnetometry projects, visit 6ccvd.com or contact our engineering team directly. Global shipping available (DDU default; DDP on request).
View Original Abstract
Nitrogen-vacancy centers in diamond have recently been established as effective sensors of the magnetization dynamics in vicinal ferromagnetic materials. We demonstrate sub-100 nm placement accuracy of nitrogen-vacancy-containing nanodiamonds and use these as local sensors that probe optically detected ferromagnetic resonance in mesoscopically patterned Permalloy islands. These measurements reveal variations in the ferromagnetic resonance signal at different sites on these structures with distinct behavior in the edge and the bulk of patterned features. These test measurements establish an easily implemented approach for spatially targeted measurements of spin dynamics in mesoscale ferromagnets. In principle, the methodology can also be extended to local studies of nanoscale ferromagnets such as single magnetic nanowires and nanoparticles.