Impact of Carbon Diffusion Induced Stress on the Properties of Diamond/GaN Heterojunctions
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Nanomaterials |
| Published | 2026-02-12 |
| Authors | Haolun Sun, Mei Wu, Peng Xu, Chao Yuan, Ling Yang |
| DOI | 10.3390/nano16040241 |
A 15 nm carbon diffusion layer lowered the effective thermal boundary resistance of a polycrystalline diamond/GaN heterostructure. It occupied part of a 40 nm SiNx interlayer. Compared with a 10 nm layer, it also increased compressive strain in the AlGaN barrier by 32%. The authors inferred a proportional gain in piezoelectric polarization and predicted an approximately 5% increase in two-dimensional electron gas sheet density. Thermal behavior was measured, while the electrical gain remained a theoretical estimate.
Carbon diffusion changed the interface structure
Section titled “Carbon diffusion changed the interface structure”Both samples used the same epitaxial stack on SiC. The stack contained a 1.4 µm GaN buffer, a 0.8 nm AlN interlayer, and a 25 nm Al0.25Ga0.75N barrier. A roughly 40 nm SiNx passivation layer was deposited by MOCVD. This layer protected the GaN surface from H2 etching during diamond growth.
During diamond growth, a double-stage process balanced etching and deposition. Plasma power density, chamber pressure, and growth temperature were varied during nucleation to control carbon diffusion. The paper does not report the exact settings for these variables. TEM and STEM showed an islandlike carbon distribution, consistent with diamond island nucleation.
Sample A contained a 15 nm carbon diffusion layer and 25 nm of remaining amorphous SiNx. Sample B contained a 10 nm diffusion layer and 30 nm of amorphous SiNx. EDS mapping found carbon, silicon, gallium, and nitrogen distributions consistent with SiC formation in the interlayer. No carbon penetration into the GaN region was detected. TEM and EDS produced consistent layer thicknesses.
Earlier studies cited by the authors associated high plasma power density and chamber pressure with carbon diffusion and localized SiC formation. The present work connects that interface transformation to stress transfer into the AlGaN/GaN heterostructure.
Transient thermoreflectance measured the thermal boundary resistance
Section titled “Transient thermoreflectance measured the thermal boundary resistance”Transient thermoreflectance measured heat transport through the diamond/SiNx/GaN stack. A 355 nm pulse laser heated the surface. A 532 nm continuous wave probe laser was coaxial with the pump and measured temperature-dependent reflectance. Au/Ti transducers on the diamond used 80 nm Au and 5 nm Ti. The measured reflectance change had a stated linear relationship with temperature change. A 400 MHz photodetector and 500 MHz digital oscilloscope recorded the thermal signal.
An analytical heat conduction model was fitted in MATLAB R2021a with global optimization. The fit extracted the effective thermal boundary resistance, or TBR. The model grouped the diamond/SiNx interface, bulk SiNx, and SiNx/GaN interface into one effective diamond/GaN TBR. The Ti layer was included in the effective Au/diamond TBR. The AlGaN barrier and GaN buffer were treated as one GaN layer.
The fit assigned a lower effective TBR to sample A than to sample B. This associates the thicker diffusion layer and thinner residual SiNx with lower thermal resistance. The accompanying text reports no numerical fitted TBR, so only the relative comparison is available.
Molecular dynamics linked crystallization to phonon coupling
Section titled “Molecular dynamics linked crystallization to phonon coupling”Classical molecular dynamics used LAMMPS to examine carbon diffusion within amorphous SiNx. The simulated amorphous layer was generated with a melt-quench protocol. Periodic boundaries applied along x and y, while z was fixed for heat-flow analysis. The model included a top SiC layer, a mixed SiC/SiNx diffusion layer, and bottom amorphous SiNx. The Lennard-Jones potential described localized SiC and amorphous SiNx interactions. The Stillinger-Weber potential described the AlGaN layer.
As carbon diffusion increased, the interlayer phonon density of states shifted toward that of SiC. The PDOS overlap with AlGaN vibrations increased, indicating stronger phonon coupling within the simulation. The authors associated this overlap with lower interfacial resistance. Under the DMM, modified phonon velocity may raise the transmission coefficient and reduce scattering probability. The simulation supports the mechanism behind the TTR trend, but provides no numerical MD TBR in the text.
Geometric phase analysis measured strain transfer
Section titled “Geometric phase analysis measured strain transfer”Geometric phase analysis measured strain from high-resolution TEM images. FFT patterns selected the strongest conjugate diffraction spots in horizontal and vertical directions. The unstrained GaN buffer served as the zero-strain reference. Strain profiles were integrated perpendicular to the interface. Values were averaged within bulk AlGaN to remove interfacial peaks.
The in-plane strain maps showed no distinct boundary or discontinuity across the heterointerface. Out-of-plane maps showed a sharp discontinuity associated with lattice mismatch and the Poisson effect. Both samples showed a localized strain peak at the immediate interface.
The dimensionless average compressive strain was -0.033 in sample A and -0.025 in sample B. The magnitude increased by 32% with stronger carbon diffusion. The result shows that diffusion-induced stress propagated into the AlGaN barrier. EDS detected no carbon in the GaN region, so the measured strain change did not coincide with carbon penetration into GaN.
Piezoelectric theory explained the predicted electrical gain
Section titled “Piezoelectric theory explained the predicted electrical gain”Piezoelectric polarization arises from lattice mismatch and strain at the heterointerface. It governs the formation and density of the two-dimensional electron gas. The measured 32% increase in strain magnitude served as the mechanical input to the authors’ piezoelectric model. The authors treated this as a proportional 32% gain in piezoelectric polarization. Accounting for dilution by spontaneous polarization, the model predicted an approximately 5% increase in 2DEG sheet density.
No direct 2DEG sheet-density measurement or HEMT electrical test was reported. The 5% gain therefore remains a prediction rather than measured device performance.
Design guidance and unresolved issues
Section titled “Design guidance and unresolved issues”The authors recommend a carbon diffusion depth of approximately 15 nm within the 40 nm SiNx interlayer. This condition produced lower effective TBR and greater barrier strain than the 10 nm comparison. The recommendation also keeps the AlGaN/GaN interface intact, with no carbon detected in GaN. These results support increasing diffusion intensity while maintaining the heterointerface.
The fitted TBR combines several interfaces, so the reduction cannot be assigned to one interface alone. Only two diffusion depths were compared. The text describes tensile stress while reporting negative compressive strain, leaving the sign convention unclear. The authors state that the datasets are not readily available because the study remains ongoing. No device-level HEMT performance or reliability measurement was reported.
For process screening, the 15 nm diffusion depth combined lower effective TBR with larger AlGaN strain in this comparison. Device qualification still requires absolute TBR measurements, direct 2DEG characterization, and electrical testing.
Materials and support
Section titled “Materials and support”Polycrystalline diamond heat-spreading films match the paper’s diamond/SiNx/GaN integration, which needs controlled carbon diffusion and Au/Ti surface transducers for TTR measurement. The diamond materials catalog from 6CCVD offers MPCVD-grown polycrystalline diamond from 0.1 to 500 micrometers and metallization with Au or Ti. The engineering support page covers custom fabrication support, and the supplier offers global shipping.
View Original Abstract
Integrating diamond with GaN provides an effective pathway to mitigate self-heating. However, the thermal boundary resistance (TBR) remains a persistent bottleneck for further heat dissipation. While carbon (C) diffusion into the SiNx interlayer is known to reduce TBR, the associated stress evolution and its impact on device performance remain underexplored. In this work, the synergistic regulation of heat transport and electrical performance induced by C diffusion was systematically investigated. Transmission electron microscopy (TEM) was employed to characterize the interfacial microstructure and the influence of C diffusion on the interface. To further assess the resulting impact on heat dissipation, transient thermoreflectance was utilized to precisely quantify the thermal transport within the heterostructures. Classical molecular dynamics (MD) simulations were then performed to analyze the underlying physical mechanisms, revealing that intensifying C diffusion increases the phonon density of states overlap and effectively reduces the TBR. Furthermore, the intrinsic stress was quantified through geometric phase analysis (GPA) based on TEM images, demonstrating that the stress induced during the diffusion process propagates to the AlGaN/GaN heterostructure. Crucially, this stress modulation enhances the piezoelectric polarization by approximately 32%, resulting in a 5% increase in the two-dimensional electron gas (2DEG) sheet density. These findings provide a comprehensive strategy for optimizing the thermal management and mechanical reliability of high-power GaN devices.
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →
Diamond Epitaxial Growth Service
View Specs →Products
View Specs →References we cover
Section titled “References we cover”- Thermal Boundary Resistance Reduction by Interfacial Nanopatterning for GaN-on-Diamond Electronics Applications
- Record-Low Thermal Boundary Resistance between Diamond and GaN-on-SiC for Enabling Radiofrequency Device Cooling
- Reducing GaN-on-diamond interfacial thermal resistance for high power transistor applications
Original source
Section titled “Original source”References
Section titled “References”- 2014 - A Survey of Wide Bandgap Power Semiconductor Devices [Crossref]
- 2006 - Present Status and Future Prospect of Widegap Semiconductor High-Power Devices [Crossref]
- 2002 - AlGaN/GaN HEMTs-An Overview of Device Operation and Applications [Crossref]
- 2008 - GaN-Based RF Power Devices and Amplifiers [Crossref]
- 2009 - High Performance and High Reliability AlGaN/GaN HEMTs [Crossref]
- 1998 - Self-Heating in High-Power AlGaN-GaN HFET’s [Crossref]
- 2018 - Accurate Measurement of Channel Temperature for AlGaN/GaN HEMTs [Crossref]
- 2005 - Diamond Semiconductor Technology for RF Device Applications [Crossref]
- 2012 - Reduced Self-Heating in AlGaN/GaN HEMTs Using Nanocrystalline Diamond Heat-Spreading Films [Crossref]