Characterization of neodymium doped calcium tungstate single crystal by Raman, IR and luminescence spectroscopy
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-01-01 |
| Journal | Science of Sintering |
| Authors | Rouaida M. Abozaid, Zorica Lazarević, Vesna Radojević, M.S. Rabasović, Dragutin Sevic |
| Institutions | FZU ‒ Institute of Physics of the Academy of Sciences of the Czech Republic, University of Belgrade |
| Citations | 13 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Research Focus: Growth and spectroscopic characterization of Neodymium-doped Calcium Tungstate (CaWO₄:Nd³⁺) single crystals for optoelectronic applications.
- Growth Method: Single crystals grown via the Czochralski method in air, utilizing melt-pulling to produce bulk samples.
- Crystal Dimensions & Quality: Produced up to 10 mm in diameter and 70 mm in length. Dislocation density observed at 638 per cm², with a Vickers microhardness of 1.5 GPa (anisotropy absent in the <001> direction).
- Spectroscopic Validation: Seven Raman-active modes and six IR-active optical modes observed, aligning with the theoretical scheelite structure. Raman analysis confirmed the S₄ point symmetry of the [WO₄]²⁻ tetrahedrons.
- Key Optical Properties: FTIR spectra identified a strong [WO₄]²⁻ stretching vibration at 862 cm⁻¹ and a Ca-O bond at 433 cm⁻¹. The estimated luminescence lifetime for the 4F3/2 → 4I9/2 transition is approximately 140 µs.
- Processing Techniques: The bulk single crystals were sectioned using a diamond saw and mechanically polished using diamond paste to achieve optical-grade surface quality for laser-induced fluorescence (LIF) measurements.
- Conclusion: The resulting CaWO₄:Nd³⁺ crystals demonstrate high crystallinity and suitable optical quality for applications in solid-state lasers, LEDs, and cryogenic scintillation detectors.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Crystal Diameter | 10 | mm | Maximum grown dimension via Czochralski method |
| Crystal Length | 70 | mm | Total length of the pulled boule |
| Growth Rate | 6.7 | mm h⁻¹ | Optimized pulling rate for melt growth |
| Critical Rotation Rate | 30 | rpm | Rotation speed during crystal pulling |
| Dislocation Density | 638 | per cm² | Measured via chemical etching (HF/CrO₃) |
| Microhardness | 1.5 | GPa | Vickers pyramid test, 4.9 N load |
| Excitation Wavelength | 532 | nm | Nd:YAG laser (second harmonic) used for PL |
| Raman Shift (4F3/2 Transition) | 912, 835, 798 | cm⁻¹ | Characteristic Raman peaks for scheelite structure |
| FTIR WO₄ Stretching | 862 | cm⁻¹ | Strong absorption peak of [WO₄]²⁻ tetrahedron |
| FTIR Ca-O Band | 433 | cm⁻¹ | Weak metal-oxygen absorption band |
| Luminescence Lifetime | 120, 140 | µs | Decay time for 4F5/2 and 4F3/2 transitions |
| Crystallographic Group | I4₁/a | - | Space group of the tetragonal scheelite phase |
Key Methodologies
Section titled “Key Methodologies”- Single Crystal Growth (Czochralski Method):
- Technique: Melt-pulling in an ambient air atmosphere.
- Parameters: Pulling rate of 6.7 mm h⁻¹, rotation rate of 30 rpm.
- Sample Preparation:
- Slicing: Cut into tiles using a diamond saw along the <001> cleavage plane.
- Polishing: Surface finishing achieved using diamond paste to prepare for optical characterization.
- Defect Analysis:
- Etching Solution: 1 part 40% HF mixed with 2 parts saturated CrO₃.
- Etch Duration: 15 minutes at room temperature.
- Microscopy: Defects observed using a Carl Zeiss Metaval metallographic microscope at 270x magnification.
- Structural Characterization:
- XRD Setup: Philips PW 1050 diffractometer, Co Kα radiation (λ = 1.54178 Å).
- Scan Parameters: 10° to 90° range, 0.05° step size, 4 s/step counting time.
- Spectroscopic Analysis:
- Raman Spectroscopy: Princeton TriVista 557 system, 532 nm Ar-ion laser excitation at 0.25 mW.
- FTIR Spectroscopy: BOMEM DA-8 spectrometer, 80-650 cm⁻¹ range, 2 cm⁻¹ resolution.
- Luminescence: Hamamatsu C4334-01 streak camera coupled with a Vibrant OPO laser system.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”This paper highlights the necessity for high-purity, mechanically robust, and highly polished diamond tooling to successfully section, process, and characterize advanced optical single crystals like CaWO₄:Nd³<up>+</up>. The precision required for diamond saw cutting and diamond paste polishing directly correlates with the need for superior diamond consumables and substrates.
- Applicable Materials:
- Optical Grade SCD (Single Crystal Diamond): As detailed in this paper, achieving Raman modes and minimizing surface defects requires flawless tooling. Our Optical Grade SCD, with surface roughness Ra < 1nm, is ideally suited for fabricating high-precision diamond saws and polishing laps required for processing fragile, brittle crystals like scheelite tungstates.
- Heavy Boron-Doped PCD (Polycrystalline Diamond): For applications involving extreme wear during the slicing of bulk crystals, our PCD offers exceptional hardness and thermal stability. We provide standard and custom polycrystalline diamond plates up to 125mm in diameter, capable of handling demanding cutting and lapping operations.
- Customization Potential:
- Custom Metalization: While this paper focuses on spectroscopic characterization, many downstream applications for CaWO₄:Nd³<up>+</up> (such as solid-state lasers and LED integrations) require metallized contacts. 6CCVD offers internal metallization capabilities using Au, Pt, Pd, Ti, W, and Cu, ensuring optimal adhesion on optical components.
- Precision Laser Cutting: For researchers requiring exact sub-millimeter dimensions from bulk boules, our custom laser cutting services allow for highly specific sample geometries that standard diamond saws may struggle to achieve without inducing micro-cracks.
- Ultra-Thin SCD Tooling: Our ability to manufacture SCD down to 0.1 µm thickness allows for the creation of ultra-sharp cutting edges, reducing chipping and improving yield when slicing materials with specific cleavage planes like the <001> plane mentioned in the paper.
- Engineering Support:
- The successful characterization of Nd³<up>+</up> luminescence relies heavily on the surface quality and orientation of the crystal. 6CCVD’s in-house PhD engineering team specializes in material selection and can assist you in choosing the correct diamond substrate or tooling specification for similar optoelectronics, scintillator, and solid-state laser projects.
- Whether you are developing new phosphors, cryogenic scintillation detectors, or laser hosts, our experts can recommend the optimal combination of SCD, PCD, or Boron-Doped Diamond to optimize your material processing and end-product performance.
- Call to Action:
- For custom specifications, metallization consultations, or material selection advice for your next optics or crystal growth project, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
The aim of the current work was to assess obtain a single crystal of calcium tungstate doped with neodymium - (CaWO4:Nd3+), and after that, the crystal was characterized with various spectroscopic methods. The single crystal was grown from the melt using the Czochralski method in air. By optimizing growth conditions, <001>-oriented CaWO4:Nd3+ crystal? up to 10 mm in diameter were grown. Number of dislocations in obtained crystal was 102 per cm2. Micro hardness was measured with the Vickers pyramid. Anisotropy in <001> direction was not observed. Selected CaWO4:Nd3+ single crystal was cut into several tiles with the diamond saw. The plates were polished with a diamond paste. The crystal structure is confirmed by X-ray diffraction. The obtained crystal w?s studied by Raman and infrared spectroscopy. Seven Raman and six IR optical active modes predicted by group theory are observed. FTIR confirmed the occurrence of all the functional groups and bonds in this material. From the FTIR spectrum, a strong peak of 862 cm-1 has been obtained due to the stretching vibration of WO42- in scheelite structure, and a weak but sharp band at 433 cm-1 has been noticed due to the metal-oxygen (Ca-O) band. Estimated luminescence lifetime of 4F5/2 - the 4I9/2 transition is about 120 ?s; estimated luminescence lifetime of 4F3/2 - the 4I9/2 transition is about 140 ?s. All performed investigations show that the obtained CaWO4:Nd3+ single crystal has good optical quality, which was the goal of this work.