Skip to content

Development of measurement technique of mass diffusion coefficient of aqueous methanol solutions in polymer electrolyte membranes based on infrared Soret forced Rayleigh scattering method using single crystal diamond window in a sample cell

MetadataDetails
Publication Date2018-01-01
JournalJournal of Thermal Science and Technology
AuthorsHiroaki Matsuura, Daichi TOKUDA, Yuji Nagasaka
InstitutionsKeio University
Citations2
AnalysisFull AI Review Included

Development of IR-SFRS Measurement Technique Using a Single Crystal Diamond Window for Diffusion Analysis in Polymer Electrolyte Membranes

Section titled “Development of IR-SFRS Measurement Technique Using a Single Crystal Diamond Window for Diffusion Analysis in Polymer Electrolyte Membranes”
  • Core Innovation: Developed an Infrared Soret Forced Rayleigh Scattering (IR-SFRS) apparatus utilizing a single crystal diamond (SCD) window to measure mass diffusion coefficients of aqueous methanol solutions in polymer electrolyte membranes (PEMs) for Direct Methanol Fuel Cells (DMFCs).
  • Key Material Achievement: Replaced a polycrystalline diamond window with a single crystal diamond window, reducing scattered probing laser light by a factor of approximately 1/150, dramatically improving signal-to-noise ratio.
  • Optical Requirements Met: The SCD window delivers high transmittance at both the heating laser wavelength (9.714 µm) and the probing laser wavelength (639 nm), while maintaining chemical stability in the acidic environment of PEMs (Nafion).
  • Measurement Precision: Achieved relative standard uncertainties between 2.5% and 5.3% for diffusion coefficient measurements in Nafion 117 at T = 298.2 K, validated against the diaphragm cell technique within 8.9% agreement.
  • Application Value: The technique enables measurement of in-plane mass diffusion in PEMs without requiring knowledge of membrane thickness and is applicable to high-concentration methanol solutions where FTIR-ATR methods fail due to membrane swelling.
  • Targeted Diffusion Pathways: Quantified mass transport phenomena (methanol crossover) that limit DMFC efficiency, supporting development of next-generation low-permeability, high-conductivity PEMs.
ParameterValueUnitContext
Heating laser wavelength (λh)9.714µmCO2 laser emission aligned to methanol CO stretching absorption
Probing laser wavelength (λp)639nmVisible laser for diffracted beam detection
SCD window thickness0.5mmIncidence-side optical window
SCD transmittance at λh (Th)71%Mid-infrared transmission
SCD transmittance at λp (Tp)70%Visible transmission
SCD scattered light intensity ratio~1/150-Compared to polycrystalline diamond window
Fringe spacing of heating laser (Λ)28.9µmSets in-plane diffusion length scale
Diffusion length scale~101µmCharacteristic in-plane mass transport length
Characteristic diffusion time (bulk)~101-102msMass diffusion relaxation timescale
Characteristic diffusion time (Nafion 117)~102msSeveral hundred milliseconds relaxation observed
Experimental temperature (T)298.2KIsothermal measurement condition
Relative uncertainty (10 wt% methanol in Nafion)3.7%Mole fraction 0.059
Relative uncertainty (20 wt% methanol in Nafion)5.3%Mole fraction 0.123
Relative uncertainty (80 wt% methanol in Nafion)2.5%Mole fraction 0.692
Relative uncertainty (10 wt% bulk solution validation)4.0%Validation against diaphragm cell technique
Relative uncertainty (80 wt% bulk solution validation)8.9%Validation against Derlacki et al. (1985)
D12 in Nafion 117 (10 wt%)3.18 × 10-10m2·s-1In-plane diffusion coefficient
D12 in Nafion 117 (20 wt%)3.39 × 10-10m2·s-1In-plane diffusion coefficient
D12 in Nafion 117 (80 wt%)6.29 × 10-10m2·s-1In-plane diffusion coefficient
D12 in bulk solution~10-9m2·s-1Order of magnitude for unconfined solutions
CO2 laser tunable range (band 1)9.183-9.733µmVariable-wavelength emission
CO2 laser tunable range (band 2)10.125-10.811µmSecondary emission band
Acousto-optic modulator coating9.7µmAnti-reflective coating optimized for heating wavelength
Cell diameter (Cu cell)Ø32mmSample cell dimensions
Nafion 117 immersion time>24hPre-measurement equilibration period
  1. Sample Preparation:

    • Immerse Nafion 117 membranes in aqueous methanol solutions (methanol >99.8%, Wako) for at least 24 hours prior to measurement.
    • Assemble PEM between two windows inside a Cu sample cell (Ø32 mm) sealed with silicone gasket and rubber closure.
  2. Optical Setup (IR-SFRS Homodyne Detection):

    • Use a half-wavelength plate to adjust polarization into an acousto-optic modulator (1209-7-1064M, Isomet) with anti-reflective coating for 9.7 µm.
    • Split the modulated heating beam with a non-polarizing beamsplitter (PIB-5005Z; Lambda Research Optics) to create two intersecting beams in the sample.
  3. Heating Laser Selection:

    • Employ a variable-wavelength CO2 laser (L20G, Access Laser Company) tunable via micrometer.
    • Select λh = 9.714 µm based on methanol CO stretching absorption (9.8 µm peak) and Nafion 117’s weaker absorption at this wavelength, maximizing the Soret effect in the sample.
  4. Probing and Detection:

    • Use a visible probing laser at λp = 639 nm to detect first-order diffracted beams.
    • Detect signals with a photomultiplier tube through a band-pass filter; amplify via I-V amplifier; record with digital oscilloscope.
    • Apply curve-fitting analysis using relaxation time constant (τD) from Eq. (2)-(3) to extract mutual mass diffusion coefficient (D12).
  5. Window Configuration:

    • Incidence side: Single crystal diamond window (Element Six 145-500-0390, 0.5 mm thickness).
    • Exit side: Quartz glass window (Th = 0%, Tp = 94%) since the heating laser does not need to transmit through it.
  6. Validation Protocol:

    • Measure aqueous methanol bulk solutions at T = 298.2 K and compare with the established diaphragm cell technique (Derlacki et al., 1985).
    • Evaluate standard uncertainties per ISO/IEC Guide 98-3:2008 (GUM).
  • Applicable Materials: This research directly validates the use of Optical Grade Single Crystal Diamond (SCD) as an infrared-transparent, chemically stable window material for precision optical measurement in acidic environments. 6CCVD’s optical-grade SCD substrates—available in thicknesses from 0.1 µm to 500 µm and with surface roughness Ra < 1 nm—provide the low-scatter, high-transmission properties demonstrated here. For applications where cost is a primary constraint and the enhanced signal-to-noise ratio of SCD is not required, our Polycrystalline Diamond (PCD) plates (polished to Ra < 5 nm for inch-size) remain a viable alternative.

  • Customization Potential: The paper specifies custom window dimensions (4.5 × 4.5 × 0.5 mm SCD window seated in a Ø32 mm Cu cell). 6CCVD routinely delivers custom-dimension SCD and PCD substrates via in-house laser cutting, including small-format optical windows. For sample cell integration, we offer custom metalization (Au, Pt, Pd, Ti, W, Cu) to facilitate brazing, soldering, or diffusion bonding of diamond windows into metallic housings such as Cu or stainless-steel sample cells.

  • Engineering Support: The transition from polycrystalline to single crystal diamond reduced scattered light by 1/150—a critical improvement for any optical system using diamond windows. 6CCVD’s in-house PhD engineering team can assist researchers in fuel cell, spectroscopy, and optical diagnostics fields with material selection: evaluating SCD versus PCD trade-offs based on scatter sensitivity, chemical compatibility (acid, base, organic solvent), and transmission wavelength range (UV to far-IR). Our team is equipped to support similar IR spectroscopy, quantum sensing, or DMFC/PEM characterization projects where diamond’s thermal conductivity and chemical inertness are advantageous.

  • Call to Action: For custom specifications, metalization consultation, or material selection guidance for your optical measurement, spectroscopy, or electrochemical cell projects, visit 6ccvd.com or contact our engineering team directly.

View Original Abstract

We have developed an experimental apparatus for the measurement of diffusion coefficient of aqueous methanol solutions in a polymer electrolyte membrane (PEM) for direct methanol fuel cells (DMFCs), based on the infrared Soret forced Rayleigh scattering (IR-SFRS) method. Because mass transport phenomena in PEMs play significant roles, evaluation and understanding of the mass diffusion in PEMs is important. In the present study, we developed a new sample cell using a single crystal diamond window, which transmits both the heating laser with the wavelength of 9.714 μm and the probing laser with the wavelength of 639 nm. The heating wavelength was selected from the emission range of a valuable-wavelength carbon dioxide laser to utilize the absorption of methanol due to CO stretching. By using a single crystal diamond window, the scattered light of the probing laser generated at the window material which causes unpreferable effects on detection signals was reduced to about 1/150, compared to a polycrystalline diamond window. To evaluate the validity of the measurement system, we carried out experiments on the aqueous methanol solutions at a temperature of T = 298.2 K. The mass diffusion coefficient of the aqueous methanol solution with the mole fraction of 0.7 measured in the present study agreed with the measured values by the diaphragm cell technique within the relative standard uncertainty of 8.9%. After the validation, we performed experiments on three concentrations of aqueous methanol solutions in a PEM of Nafion 117 at T = 298.2 K. The mass diffusion in Nafion was observed in several hundreds of milliseconds. We obtained the mass diffusion coefficient with the relative standard uncertainties of 2.5-5.3%, depending on the methanol concentration. The mass diffusion coefficient in Nafion 117 was smaller than that of bulk aqueous methanol solutions, and increased with the increase in the methanol mole fraction.