Skip to content

Fluorescent Fe Embedded Magnetic Nanodiamonds Made by Ion Implantation

MetadataDetails
Publication Date2019-02-04
JournalScientific Reports
AuthorsBo-Rong Lin, Srinivasu Kunuku, C.H. Chen, Tzung-Yuang Chen, Tung‐Yuan Hsiao
InstitutionsNational Yang Ming Chiao Tung University, National Tsing Hua University
Citations11
AnalysisFull AI Review Included

Dual-Function Fluorescent Magnetic Nanodiamonds via Ion Implantation: Technical Analysis

Section titled “Dual-Function Fluorescent Magnetic Nanodiamonds via Ion Implantation: Technical Analysis”
  • Core Innovation: Fabrication of dual-function in vivo tracer nanoparticles combining magnetic resonance imaging (MRI) contrast and red fluorescence (≈680 nm) imaging in a single nanodiamond (ND) platform.
  • Material Strategy: Commercial ND powder (≈100 nm diameter, Microdiamant Co.) used as the host lattice; ion implantation used to embed iron (Fe) atoms directly into the sp3 carbon core rather than attached to the surface.
  • Process Architecture: High-energy Fe-ion implantation (150 keV, 5 × 1015 ions/cm2) combined with a two-step annealing protocol to simultaneously generate NV centers and remove graphitic sp2 surface contamination.
  • Key Achievement: Bright red fluorescence (≈700 nm) detectable via both photoluminescence (PL) spectroscopy and IVIS imaging systems — confirming optical visibility alongside magnetic functionality.
  • Critical Insight: Both ion implantation AND two-step annealing are mandatory; neither step alone yields detectable fluorescence under bio-imaging conditions.
  • End-Use Value: Biocompatible nano-tracer enabling fluorescence imaging in optically accessible tissues and MRI in deeper regions, eliminating the cytotoxicity concerns of surface-bound iron compounds.

ParameterValueUnitContext / Notes
Starting ND Diameter~100nmMicrodiamant Co. commercial powder
Fe-Ion Implantation Energy150keVAccelerates Fe into diamond bulk
Fe-Ion Dose5 × 1015ions/cm2High-dose bombardment
First Anneal Temperature800°CVacuum environment
First Anneal Duration2hNV center formation step
Second Anneal Temperature450°CAir (oxidizing) environment
Second Anneal Duration3hGraphite layer removal step
Fluorescence Peak Wavelength~680-700nmRed emission, NV0/NV- centers
Surface Layer After ImplantFew nmnmGraphitic sp2 shell around sp3 core
PL Radiant Efficiency Range1.2 × 106 - 6.4 × 106a.u.Two-step annealed Fe-NDs (IVIS)
Imaging ModalityMRI + Fluorescence—Dual-function tracer

  1. Substrate Preparation
    • Disperse ~100 nm ND powder (Microdiamant) in deionized water.
    • Coat uniformly onto an oxidized silicon wafer.
  2. Fe-Ion Implantation
    • Energy: 150 keV.
    • Dose: 5 × 1015 ions/cm2.
    • Purpose: Embed Fe atoms inside ND lattice; create carbon vacancies.
  3. Magnetic Collection
    • Collect Fe-implanted magnetic NDs from suspension.
    • Re-disperse onto fresh silicon wafer for thermal processing.
  4. Two-Step Annealing Protocol
    • Step 1 (NV Formation): 800 °C for 2 h in vacuum → mobilizes vacancies, enabling combination with substitutional N to form NV emission centers.
    • Step 2 (Surface Cleanup): 450 °C for 3 h in air → selectively oxidizes and removes graphitic sp2 shell that otherwise quenches fluorescence.
  5. Characterization Pipeline
    • TEM imaging for structural integrity verification.
    • EDS mapping for Fe spatial distribution confirmation.
    • PL spectroscopy (600-800 nm range) for NV emission analysis.
    • IVIS fluorescence imaging for macroscopic luminescence validation.

The research outlined here hinges on a precise combination of factors: ultra-pure diamond lattice integrity, controlled defect engineering, and clean surface chemistry. Translating this to high-purity MPCVD-grown material requires deliberate material selection and post-processing capability.

  • Optical-Grade Single Crystal Diamond (SCD): Optimal for any extension of this work that requires well-defined NV center physics. 6CCVD’s SCD can be grown with controlled nitrogen incorporation to provide the substitutional N needed for NV formation, while minimizing background impurities.
  • High-Purity Polycrystalline Diamond (PCD): Suitable for scaled-down, cost-sensitive bio-imaging tracer development. Available in thicknesses from 0.1 µm to 500 µm, enabling powder-like or thin-film experimental geometries.
  • Boron-Doped Diamond (BDD): Relevant if subsequent research explores conductive pathways for combined magnetometry/electrochemical biosensing extensions.
  • Substrate & Wafer Geometry: Although this work used 100 nm powder, scaling to planar devices or test-patterned chips is fully within 6CCVD’s capability. Custom plates and wafers are produced up to 125 mm diameter.
  • Ion-Implantation-Ready Surface Finishes: Surface polishing is offered to Ra < 1 nm (SCD) and < 5 nm (inch-size PCD). Sub-nanometer surface roughness is critical for clean Fe-ion penetration profiles and reproducible NV yield.
  • Custom Metalization & Laser Cutting: Should the project evolve into electrode-integrated NV sensors or on-chip arrays, 6CCVD provides in-house Au, Pt, Pd, Ti, W, and Cu metalization, plus laser cutting for precise geometries.
  • Thickness Tuning for Ion Range Engineering: SCD thicknesses from 0.1 µm to 500 µm (and substrates up to 10 mm) allow researchers to align the stopping range of implanted ions with intended NV-active layers.

The interplay between implantation energy, vacancy density, and annealing atmosphere is non-trivial. 6CCVD’s in-house PhD engineering team provides material consultation for biomedical and quantum-sensing projects, including:

  • Recommendation of starting nitrogen concentration in SCD/PCD to optimize NV density per implanted Fe dose.
  • Surface preparation guidance (hydrogen-terminated vs. oxidized) for downstream bio-functionalization.
  • Discussion of polishing protocols that minimize sub-surface damage — critical for preserving spin coherence in NV-based sensing.

For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.

View Original Abstract

We demonstrate fluorescent Fe embedded magnetic nanodiamonds by ion implantation and two-step annealing. The diamond characteristics with a highly ordered core and a graphite surface layer are maintained after the implantation process. After the two-step annealing process, a bright red fluorescence associated with nitrogen-vacancy centers is observed. These new fluorescent magnetic nanodiamonds can be used as a dual-function in vivo tracer with both optical visibility and magnetic resonance imaging capabilities. They are potentially useful for the more advanced in vivo biological and medical applications.