Smart Cut™ technology for the integration of diamond Schottky diodes on silicon substrate
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Applied Physics Letters |
| Published | 2026-07-13 |
| Authors | J. Chrétien, R. Gourad, H. Soares-Antunes, P. Gilles, C. Masante |
| DOI | 10.1063/5.0334593 |
Functional p-type pseudo-vertical diamond Schottky diodes were fabricated on a Smart Cut™ transferred diamond-on-silicon stack. Across 13 devices, the reported forward current density was 25 A cm⁻² at 5 V. Rectification extended between -5 V and 20 V, with blocking above 100 V. The 500 nm transferred film also supported boron-doped regrowth before aluminum Schottky contacts were fabricated on silicon.
Transfer and epitaxial regrowth
Section titled “Transfer and epitaxial regrowth”Smart Cut used a 4 × 4 mm² CVD heteroepitaxial single-crystal diamond donor. Hydrogen implantation and annealing created a graphite-like buried layer at 750 nm. Surface activated bonding joined the donor to silicon. A later anneal produced hydrogen-pressurized microcracks and split the donor along that layer.
The transfer initially left 750 nm of diamond with inverted pyramids. Sulfuric acid and potassium nitrate removed residual graphite-like material. Ar/O₂ RIE removed 250 nm of defective top material. The remaining 500 nm film had 0.1 nm root mean square roughness over locally smooth areas and was ready for epitaxial growth.
Two homoepitaxial layers were grown in separate NIRIM-type microwave plasma chemical vapor deposition reactors. Before p layer growth, an in situ hydrogen plasma cleaned the surface and slightly etched the p++ layer at dislocation sites.
| Layer | Thickness | Temperature | Pressure | Gas and dopant |
|---|---|---|---|---|
| Heavily boron-doped p++ | 9 μm | 850 °C | 80 mbar | 2% CH₄/H₂, trimethylboron/H₂ at 0.1%, target 2 × 10²⁰ cm⁻³ |
| p active layer | 4 μm | 850 °C | 100 mbar | 1% CH₄/H₂, not intentionally doped |
The pyramid morphology came from silicon’s brittle-to-ductile transition during splitting, not from epitaxial growth. The final surface had no hillocks.
Diode fabrication
Section titled “Diode fabrication”A silicon mask protected the Schottky contact while selected areas were exposed for a 5 μm selective RIE. The etch reached the p++ layer and created openings for ohmic contacts.
Evaporation through a hard mask formed 300 nm aluminum circular pads with a diameter of 280 μm. The aluminum formed the p++ ohmic contact and the p layer Schottky contact. SEM and profilometry confirmed a total diamond stack thickness of 14 μm.
Crystal quality and doping
Section titled “Crystal quality and doping”Heavy boron doping produced Fano interference in the p++ Raman spectrum. The zone-center optical phonon near 1330 cm⁻¹ shifted and broadened. Broad bands near 510 and 1220 cm⁻¹ arose from interaction between the electronic continuum and diamond phonons. Raman fitting gave a p++ doping concentration of 1.3 to 9.9 × 10²⁰ cm⁻³.
The p layer showed a sharp diamond peak at 1333 cm⁻¹ and no D or G bands near 1350 and 1580 cm⁻¹. This combination supported high crystallinity and a well ordered sp³-bonded carbon structure. Weak broad signals were attributed to the underlying p++ layer under 532 nm excitation.
Capacitance-voltage measurements at 500 kHz extracted the effective p layer doping. The profile gave 6.4 × 10¹⁵ cm⁻³ at 0.8 μm and 2 × 10¹⁶ cm⁻³ at 2.4 μm. Measurements below 0.8 μm were limited by the onset of conduction.
A 100 kHz map near 0 V at 0.8 μm gave an average of 5.2 × 10¹⁵ cm⁻³. Its standard deviation was 7.7 × 10¹⁴ cm⁻³. The authors proposed residual boron contamination. Hydrogen plasma etching may have shortened the active layer from 4 μm to about 2.5 μm, but they did not confirm that mechanism.
Room temperature electrical performance
Section titled “Room temperature electrical performance”| Electrical result | Value | Condition |
|---|---|---|
| Forward current density | 25 A cm⁻² | Room temperature, 5 V |
| Average differential specific on-resistance | 157 mΩ cm² | Room temperature |
| Average reverse leakage density | 1.3 × 10⁻⁷ A cm⁻² | Room temperature, 20 V |
| Average Schottky barrier height | 0.84 eV | Room temperature, thermionic fit from 0.25 to 1 V |
| Average ideality factor | 1.60 | Room temperature, thermionic fit from 0.25 to 1 V |
Most of the 13 diodes rectified between -5 V and 20 V at room temperature. The paper’s abstract gives a rectifying ratio of 10⁶, while its detailed current-voltage discussion reports seven orders of magnitude.
Thermionic emission was fitted from 0.25 to 1 V with the Richardson constant set to 90 A cm⁻² K⁻². The extracted barrier was lower than 1.05 eV and 1.13 eV from earlier studies. The ideality factor ranged from 1 to 2.
At 100 V, leakage reached 7.2 × 10⁻⁶ A cm⁻². With a 2.5 μm depleted layer, the estimated average reverse field was 0.4 MV/cm, and the maximum was 0.7 MV/cm. Possible causes identified by the authors were defects from the donor, transfer, or p++ layer, and incomplete depletion.
Early lateral diamond Schottky diodes reported breakdown voltages of 6.7 to 12 kV and operation at 700 °C. Their low boron doping caused high series resistance. Earlier pseudo-vertical diodes were limited to 2.1 to 2.7 MV/cm. One reported 7.7 MV/cm with 10³ A cm⁻² at 6 V. Heteroepitaxial Schottky diodes were reported at 1 to 2 MV/cm. The present current density and average field fall below those reference results.
High temperature behavior
Section titled “High temperature behavior”A tested diode retained rectification up to 175 °C. It no longer operated above that temperature. The temperature-dependent Richardson plot gave a constant of 0.0318 A cm⁻² K⁻² and a barrier height of 0.72 eV.
The authors linked the departure from ideal thermionic emission to possible barrier inhomogeneity, an insulating interlayer, or other transport mechanisms. They identified sp² clusters, dislocations, surface termination, and nonuniform doping as sources of barrier variation. Frenkel-Poole emission, variable range hopping, and phonon-assisted tunneling were also possible. Electric field and temperature studies are needed to separate these mechanisms.
Limits and proposed improvements
Section titled “Limits and proposed improvements”The device data are preliminary. The authors said better surface treatment and a more suitable Schottky metal, such as zirconium on oxygen-terminated diamond, may improve performance. They also called for investigation of the crystalline quality of the regrown layers.
A comparison of devices made directly on the donor and receiver substrates could isolate the defect effects. The comparison would cover the heteroepitaxial donor, Smart Cut transfer, and p++ regrowth. They proposed using homoepitaxial or HPHT substrates for future Smart Cut transfers to reduce defects.
Another transfer design would place a heavily doped p++ layer on a p-type substrate. This would prevent defect propagation from the heavily boron-doped substrate into the active layer.
Device engineering implications
Section titled “Device engineering implications”The process shows that thin single-crystal diamond can be regrown and device processed on silicon using industrial cleanroom steps. Existing heteroepitaxial diamond substrates reached 90 mm. Smart Cut could reduce cost compared with bulk diamond substrates and enable larger wafers through surface tiling. The authors present larger-wafer production as a future possibility.
For device selection, the measured forward density, blocking voltage, and average field should be treated as the present baseline. Donor crystal quality, regrowth defects, boron uniformity, surface termination, and the metal interface must be considered for higher-field operation.
Materials and support
Section titled “Materials and support”The paper uses a boron-doped single-crystal p++ layer and a p-type active layer after a 500 nm Smart Cut transfer film for its p-type Schottky barrier diode. 6CCVD’s diamond materials catalog lists single-crystal diamond grown by MPCVD and boron-doped diamond, with plates and wafers up to 125 mm and thickness from 0.1 to 500 μm. The paper’s Al contact scheme is not among the listed Au, Pt, Pd, Ti, W, and Cu options, so it needs separate review through engineering support.
View Original Abstract
Diamond is a promising candidate for next-generation high-power electronic devices due to its exceptional thermal and electrical properties. This work demonstrates homoepitaxial regrowth on Smart Cut™ transferred diamond-on-Si substrates and the subsequent fabrication of electronic devices. Specifically, heavily p-doped (p++) and p-doped diamond layers were sequentially grown onto a 500 nm single-crystal heteroepitaxial diamond film that had been transferred to a silicon substrate via the Smart Cut™ process. Functional pseudo-vertical Schottky barrier diodes were successfully fabricated using aluminum contacts. Raman spectroscopy and capacitance-voltage measurements confirmed doping concentrations of 2×1020 and 1×1015 cm−3 for the p++ and p-doped layers, respectively. Current-voltage (I-V) characterization revealed robust rectification behavior, featuring a forward current density of 25 A cm−2 (at −5 V), a rectifying ratio of 106, and a breakdown voltage above 100 V (corresponding to an average electric field of 0.4 MV/cm). These results validate the viability of Smart Cut™ diamond-on-silicon as a scalable platform for advanced diamond power electronics.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Boron Doped Single Crystal Diamond Plate
View Specs →
Diamond Epitaxial Wafer For Diodes 2
View Specs →References we cover
Section titled “References we cover”- Pseudovertical Schottky Diodes on Heteroepitaxially Grown Diamond
- Growth defects in heteroepitaxial diamond
- Influence of Different Surface Morphologies on the Performance of High-Voltage, Low-Resistance Diamond Schottky Diodes
Original source
Section titled “Original source”References
Section titled “References”- 2003 - Exceptionally high voltage Schottky diamond diodes and low boron doping [Crossref]
- 2004 - High-voltage diamond Schottky rectifiers
- 2009 - Low-leakage p-type diamond Schottky diodes prepared using vacuum ultraviolet light/ozone treatment [Crossref]
- 2010 - Extreme dielectric strength in boron doped homoepitaxial diamond [Crossref]
- 2011 - Schottky diode architectures on p-type diamond for fast switching, high forward current density and high breakdown field rectifiers [Crossref]
- 1998 - High temperature, high voltage operation of diamond Schottky diode [Crossref]
- 2014 - Zr/oxidized diamond interface for high power Schottky diodes [Crossref]
- 2020 - Influence of different surface morphologies on the performance of high-voltage, low-resistance diamond Schottky diodes [Crossref]
- 2013 - Vertical diamond Schottky barrier diode fabricated on insulating diamond substrate using deep etching technique [Crossref]
- 2013 - 1 Ω on-resistance diamond vertical-Schottky barrier diode operated at 250 °C [Crossref]